[0013] (1) Preparation of solution: Add 30g of mercaptoacetic acid, 2g of lithium chloride and 3g of sodium lauryl sulfate into 100ml of water to form a mixed solution, adjust the pH value to 9-10 with sodium hydroxide, and then add Add 0.3g nano-graphite powder in, obtain the dissolving solution that is dispersed with nano-graphite powder under ultrasonic vibration;
[0014] (2) padding the woolen fabric in the solution solution obtained in step (1) several times, and the excess rate is 70%;
[0015] (3) Steam the wool fabric after padding at 120°C for 10 minutes;
[0016] (4) Soak the steamed wool fabric in an aqueous solution of polyvinyl alcohol (12% by mass) to solidify for 10 minutes, then wash and dry.
Embodiment 2
[0018] (1) Preparation of solution: Add 40g of mercaptoacetic acid, 2g of lithium chloride and 3g of sodium lauryl sulfate into 100ml of water to form a mixed solution, adjust the pH value to 9-10 with sodium hydroxide, and then add Add 0.6g nanometer carboxylated graphene in, obtain the dissolving solution that is dispersed with nanometer carboxylated graphene under ultrasonic vibration;
[0019] (2) padding the woolen fabric in the solution solution obtained in step (1) several times, and the excess rate is 100%;
[0020] (3) Steam the padded wool fabric at 120°C for 8 minutes;
[0021] (4) Soak the steamed wool fabric in an aqueous solution of polyvinyl alcohol (14% by mass) to solidify for 10 minutes, then wash and dry.
Embodiment 3
[0023] (1) Preparation of solution: Add 45g of mercaptoacetic acid, 3g of lithium chloride and 4g of sodium lauryl sulfate into 100ml of water to form a mixed solution, adjust the pH value to 9-10 with sodium hydroxide, and then add Add 0.8g of carbon nanotubes to the solution, and obtain a solution in which carbon nanotubes are dispersed under ultrasonic vibration;
[0024] (2) padding the woolen fabric in the solution obtained in step (1) several times, and the excess rate is 110%;
[0025] (3) Steam the padded wool fabric at 110°C for 25 minutes;
[0026] (4) Soak the steamed wool fabric in an aqueous solution of polyvinyl alcohol (18% by mass) to solidify for 10 minutes, then wash and dry.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com