Preparation method of low-slagging sludge biomass solid fuel
A technology for solid fuel and biomass, which is applied in the field of low-slagging sludge biomass solid fuel preparation, can solve the problems of large slagging amount and affecting the combustion effect of dyes, and achieves hard slagging, remarkable combustion effect, and avoidance of silicon dioxide. The effect of acid formation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A preparation method of low-slagging sludge biomass solid fuel, comprising the following operation steps:
[0016] (1) Add the modified liquid to the sludge, adjust the sludge into a slurry with a mass moisture content of 91%, and obtain a modified sludge, wherein the modified liquid is made of the following components by weight: methyl propylene sulfonic acid 14 parts of sodium, 3 parts of sodium molybdate dihydrate, 1 part of o-hydroxybenzoic acid, 16 parts of potassium hydrogen phthalate, 25 parts of sodium lignosulfonate, and 850 parts of water;
[0017] (2) The dried crop straws were pulverized to an average length of 1 cm to obtain broken straws, and then, in parts by weight, 89 parts of modified sludge, 33 parts of broken straw, 0.1 part of sodium orthovanadate, 0.1 part of The igniter, after mixing and stirring evenly, is added to the filter press to obtain low-slagging sludge biomass solid fuel.
[0018] Specifically, in the above step (1), the initial moistur...
Embodiment 2
[0022] A preparation method of low-slagging sludge biomass solid fuel, comprising the following operation steps:
[0023] (1) Add a modified liquid to the sludge, and prepare the sludge into a slurry with a mass moisture content of 93% to obtain a modified sludge, wherein the modified liquid is made of the following components by weight: methyl propylene sulfonic acid 16 parts of sodium, 5 parts of sodium molybdate dihydrate, 2 parts of o-hydroxybenzoic acid, 18 parts of potassium hydrogen phthalate, 28 parts of sodium lignosulfonate, 880 parts of water;
[0024] (2) The dried crop straws are pulverized to an average length of 1.5cm to obtain broken straws, and then, in parts by weight, 92 parts of modified sludge, 36 parts of broken straws, 0.2 parts of sodium orthovanadate, 0.1 After mixing and stirring evenly, it is added to the filter press to obtain low-slagging sludge biomass solid fuel.
[0025] Specifically, in the above step (1), the initial moisture content of the s...
Embodiment 3
[0029] A preparation method of low-slagging sludge biomass solid fuel, comprising the following operation steps:
[0030] (1) Add a modified liquid to the sludge, and prepare the sludge into a slurry with a mass moisture content of 95% to obtain a modified sludge, wherein the modified liquid is made of the following components by weight: methyl propylene sulfonic acid 18 parts of sodium, 8 parts of sodium molybdate dihydrate, 3 parts of o-hydroxybenzoic acid, 20 parts of potassium hydrogen phthalate, 30 parts of sodium lignosulfonate, and 900 parts of water;
[0031] (2) Pulverize the dried crop straws to an average length of 2 cm to obtain broken straws, and then, in parts by weight, 95 parts of modified sludge, 40 parts of broken straws, 0.3 parts of sodium orthovanadate, 0.2 parts of The igniter, after mixing and stirring evenly, is added to the filter press to obtain low-slagging sludge biomass solid fuel.
[0032] Specifically, in the above step (1), the initial moisture...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com