A filter cake and waste liquid technology, applied in the field of joint disposal of high rhenium arsenic filter cake and copper-containing waste liquid and extraction of rhenium from high rhenium arsenic filter cake, can solve the problems of complex process, difficult stripping, long process and so on , to achieve the effect of simplifying the process flow, eliminating purification steps, and facilitating crystallization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] a), Purify the smelting flue gas containing arsenic and rhenium in the flue gas purification system, set the cleaning cycle of the filter layer in the purification system to 10 days, and use the diacetyl arsenic filter cake obtained by diacetyl oxime spectrophotometry Measure the content of rhenium in the gained arsenic filter cake to be 1.16%;
[0028] b) Add the arsenic filter cake containing 1.16% rhenium and the sulfuric acid leaching solution of copper anode slime containing 1% copper obtained in step a) into the leaching tank at a liquid-solid ratio of 3:1, and mix and leaching under normal pressure and 60°C After 2 hours, the obtained mixed leachate was subjected to solid-liquid separation to obtain leachate B1 and leach residue B2;
[0029] c) The leaching solution B1 adsorbs rhenium through the ion exchange resin to obtain the ion exchanged liquid C1. When the ion exchange resin is close to saturation, backwash and desorb the ion exchange resin with ammonia sol...
Embodiment 2~9
[0034] Embodiment 2~9 are identical with embodiment 1 step, and process parameter is as shown in table 1:
[0035] From the data obtained in the above 9 examples, it can be known that the method for extracting rhenium in combination with the high-rhenium-arsenic filter cake and copper-containing waste liquid of the present invention, when the smelting flue gas continues to pass through the flue gas purification system, after setting the cleaning cycle of the filter layer, The fluctuation of rhenium content in the obtained high-rhenium-arsenic filter cake is very small, which provides convenience for determining the time required for subsequent control of each part of the technological process. The measured concentration of the recovered dilute sulfuric acid is about 20-30%. Returning to the leaching step for recycling can meet the requirements of the leaching process for the concentration of the leaching solvent; the calculated comprehensive recovery rate of rhenium can reach m...