A porous ceramic for an electronic cigarette atomizer and its preparation method, and an electronic cigarette with the porous ceramic for an electronic cigarette atomizer

An electronic cigarette atomizer and porous ceramic technology, applied in the field of electronic cigarettes, can solve the problems of uncontrollable distribution of pore size, poor strength, easy drop of fine particles, etc.

Active Publication Date: 2021-09-10
NINGBO TOPTEK ADVANCED CERAMICS CO LTD
View PDF5 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0005] However, porous ceramics used as smoke oil absorbers generally require a higher oil absorption rate of the porous ceramics, so that the smoke produced by atomization will be more
However, after the ceramic has a large porosity and a larger pore size, first, the strength will deteriorate, and fine particles will easily fall off the ceramic body. If it is inhaled into the mouth, it will seriously affect the experience of using the electronic cigarette.
The second is that the pore size distribution is often uncontrollable. After the oil absorption rate increases, the oil locking ability will decrease, and oil leakage is prone to occur, which will cause liquid e-liquid to enter the mouth of the smoker, affecting the taste and experience
If the porosity is too small, the oil conductivity will decrease, the amount of smoke will decrease, which will also affect the experience, and the wettability of the e-liquid to porous ceramics is not good enough, which will also affect the oil absorption speed

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A porous ceramic for an electronic cigarette atomizer and its preparation method, and an electronic cigarette with the porous ceramic for an electronic cigarette atomizer

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0043] Method for preparing electronic cigarette porous ceramic, including the following steps:

[0044] Step 1, 80kg of diatomaceous earth in natural porous materials, the average aperture of diatomite is 5 um, and it is added to the mixer, then the particle size is 300 mesh pure agent graphite powder 20 kg, and then diatomaceous earth and graphite The powder is mixed and mixed, and the powder is obtained;

[0045] Step 2, mix the uniform powder in the step one is placed in the rubber sleeve, and the sealing is sealed in the cold and equal pressure press, and the pressure is controlled at 100 MPa, pressurized for 10 minutes, and then pressed the crimped blank.

[0046] Step three, put the blank into the heating furnace, heated to 1200 ° C at a heating rate of 1 ° C / min, and heat the aperture agent in the blank, thereby obtaining a porous ceramic skeleton preform.

[0047] Step 4. Use a roller ball mill to break the obtained porous ceramic skeleton prefabricate, and select the s...

Embodiment 2

[0055] Method for preparing electronic cigarette porous ceramic, including the following steps:

[0056] Step 1, 50 kg of diatomaceous earth in natural porous material, the average aperture of diatomaceous earth is 200 um, and it is added to the mixer, and then the particle size is 100 megadownload mesh charcoal, which will be added to 50 kg, and then briquette and graphite powder. The aperture is mixed and mixed, and the powder is obtained;

[0057] Step 2, the mixed powder in the step one is placed in the rubber sleeve, and the sealing is sealed in the cold and equal static press, the pressure is controlled at 50 MPa, pressurized for 2 minutes, and then pressed the crimped blank.

[0058] Step three, placing the blank into the heating furnace, heating to 700 ° C at a heating rate of 5 ° C / min, heat insulation for 1 hour, and is completely burned, thereby obtaining a porous ceramic skeleton preform.

[0059] Step 4. Use a roller ball mill to break the obtained porous ceramic sk...

Embodiment 3

[0067] Method for preparing electronic cigarette porous ceramic, including the following steps:

[0068] A step of, natural selection Celite 60Kg porous material, the average pore diameter is 100um diatomaceous earth, which was added to the mixer, and then added to a particle size of 200 mesh 40Kg pore-forming agent cellulose, diatomaceous earth and graphite after The powder is mixed and mixed, and the powder is obtained;

[0069] Step 2, mix the uniform powder in step one, in the rubber sleeve, sealed in the cold and dispersion machine, and the pressure is controlled at 80 MPa, pressed for 8 minutes, then taken out the crimped blank.

[0070] Step three, placing the blank into the heating furnace, heated to 950 ° C at a heating rate of 3 ° C / min, and heat it for 3 hours, and the aperture in the blank is completely burned, thereby obtaining a porous ceramic skeleton preform.

[0071] Step 4. Use a roller ball mill to break the obtained porous ceramic skeleton prefabricate, and s...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a porous ceramic for an electronic cigarette vaporizer, which relates to the field of electronic cigarettes and comprises the following components in parts by mass: 50-80 parts of diatomite, 5.35-12.2 parts of boron oxide and 2.15-2.15 parts of aluminum dihydrogen phosphate 9.8 servings. Due to the addition of boron oxide and aluminum dihydrogen phosphate, the compressive strength of porous ceramics is effectively improved. The preparation method mainly includes mixing diatomite and pore-forming agent, making compact, firing porous ceramic skeleton prefabricated body, crushing porous ceramic skeleton prefabricated body, preparing porous ceramic powder, preparing mud, forming porous ceramic oil-conducting Rods, sintered semi-finished porous ceramics, and semi-finished porous ceramics are coated with a silane coupling agent to obtain finished products. The uniform distribution of pores inside the porous ceramic is achieved by this method, thereby improving the ability of absorbing and locking oil. Moreover, the porous ceramic electronic cigarette of the present application gives users a good sense of experience.

Description

Technical field [0001] The present invention relates to the field of field of electronic cigarettes, and more particularly, it relates to an electronic smoke uniform porous ceramic and a preparation method thereof and an electronic cigarette with the electron smoke makeup. Background technique [0002] Electronic cigarettes are a use of a rechargeable lithium polymer battery to generate a smoke through heating "smoke bomb", which replaces new products of traditional cigarettes. Electronic cigarettes are harmful to the human body less than traditional cigarettes, and the electronic cigarettes are not involved in the process of smoke, and there are hundreds of harmful substances such as tar in traditional cigarette combustion. [0003] The atomizer is the core component of the electronic cigarette. At present, the mainstream structure is a glass fiber rope as a conductive medium, and the glass fiber rope is wrapped around a circle heating resistant wire. When working, the battery r...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C04B35/14C04B38/08C04B38/06C04B41/84A24F47/00
CPCC04B35/14C04B38/08C04B41/009C04B41/4905C04B41/84C04B2235/96C04B2235/447C04B2235/3409C04B38/068C04B38/0054C04B38/0645
Inventor 杨辉罗杰锋龚晶晶
Owner NINGBO TOPTEK ADVANCED CERAMICS CO LTD
Features
  • R&D
  • Intellectual Property
  • Life Sciences
  • Materials
  • Tech Scout
Why Patsnap Eureka
  • Unparalleled Data Quality
  • Higher Quality Content
  • 60% Fewer Hallucinations
Social media
Patsnap Eureka Blog
Learn More