Box culvert polymer compression molding material
A polymer and injection technology, applied in solid waste management, sustainable waste treatment, climate sustainability, etc., can solve problems such as inability to strengthen and repair structures, reduce land acquisition, reduce risks, ensure stability and long lasting effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0047] A new type of modified urban drainage pipe and box culvert non-excavation structure reinforcement and repair material--the production method of box culvert polymer pressure injection material:
[0048] First grind the polymer, modified composite mineral powder, and quartz powder according to the mass ratio of 1:3:1, the fineness is: 1000 mesh, and then mix the ground masterbatch with cement, concrete expansion agent, quartz sand, The water agent is used to prepare box culvert polymer injection material at a weight ratio of 1:4:0.24:4.73:0.03, put the prepared injection material into a twin-shaft mixer and stir for 10 minutes, and seal the package after stirring evenly.
[0049] The polymer is redispersed latex powder 5044N.
[0050] The preparation method of the modified composite mineral powder is:
[0051] Mix coal gangue powder with a particle size of 100-150 mesh: kaolin powder: tourmaline powder: rice husk incineration powder = 1:2:2:0.2, add water 5 times the tot...
Embodiment 2
[0054] A new type of modified urban drainage pipe and box culvert non-excavation structure reinforcement and repair material--the production method of box culvert polymer pressure injection material:
[0055] First grind the polymer, modified composite mineral powder, and quartz powder according to the mass ratio of 1:3:1, the fineness is: 1000 mesh, and then mix the ground masterbatch with cement, concrete expansion agent, quartz sand, The water agent is used to prepare box culvert polymer injection material at a weight ratio of 1:4:0.24:4.73:0.03, put the prepared injection material into a twin-shaft mixer and stir for 10 minutes, and seal the package after stirring evenly.
[0056] The polymer is redispersed latex powder 5044N.
[0057] As preferably, the preparation method of the modified composite mineral powder is:
[0058] Mix coal gangue powder with a particle size of 100-150 mesh: kaolin powder: tourmaline powder: rice husk incineration powder = 1:2:2.2:0.2, add wate...
Embodiment 3
[0061] A new type of modified urban drainage pipe and box culvert non-excavation structure reinforcement and repair material--the production method of box culvert polymer pressure injection material:
[0062] First grind the polymer, modified composite mineral powder, and quartz powder according to the mass ratio of 1:3:1, the fineness is: 1000 mesh, and then mix the ground masterbatch with cement, concrete expansion agent, quartz sand, The water agent is used to prepare box culvert polymer injection material at a weight ratio of 1:4:0.24:4.73:0.03, put the prepared injection material into a twin-shaft mixer and stir for 10 minutes, and seal the package after stirring evenly.
[0063] The polymer is redispersed latex powder 5044N.
[0064] As preferably, the preparation method of the modified composite mineral powder is:
[0065] Mix coal gangue powder with a particle size of 100-150 mesh: kaolin powder: tourmaline powder: rice husk incineration powder = 1:2:2.5:0.2, add 5 ti...
PUM
| Property | Measurement | Unit |
|---|---|---|
| minimum film forming temperature | aaaaa | aaaaa |
| particle size (mesh) | aaaaa | aaaaa |