Embodiment 1
[0040] An environmentally friendly marine anti-corrosion coating suitable for large ships, consisting of the following components by weight percentage:
[0041] Epoxy 18%
[0042] Ultrafine Barium Sulfate 6%
[0043] Light Calcium Carbonate 10%
[0044] Thixotropic agent 2%
[0045] Curing agent 7%
[0046] Film-forming catalyst 0.15%
[0047] Algaecide 1.5%
[0048] Dispersant 1.5%
[0049] Amine resin 28%
[0050] Nano silica 0.07%
[0051] Toner 6%
[0052] Silica powder balance.
[0053] The particle diameter of the silicon micropowder is 800 mesh, the particle diameter of the ultrafine barium sulfate is 500 mesh, and the nano silicon dioxide.
[0054] The thixotropic agent is organic bentonite.
[0055] The curing agent is an organic acid curing agent.
[0056] The film-forming catalyst is lanthanum oxide.
[0057] The epoxy equivalent of the epoxy resin is 3000-4500g / eq.
[0058] The amine resin is bismaleimide resin.
Embodiment 2
[0060] An environmentally friendly marine anti-corrosion coating suitable for large ships, consisting of the following components by weight percentage:
[0061] Epoxy 25%
[0062] Ultrafine Barium Sulfate 5%
[0063] Light Calcium Carbonate 12%
[0064] Thixotropic agent 1%
[0065] Hardener 10%
[0066] Film-forming catalyst 0.1%
[0067] Algaecide 3%
[0068] Dispersant 1%
[0069] Amine resin 35%
[0070] Nano silica 0.05%
[0071] Toner 8%
[0072] Silica powder balance.
[0073] The particle diameter of the silicon micropowder is 800 mesh, the particle diameter of the ultrafine barium sulfate is 500 mesh, and the nano silicon dioxide.
[0074] The thixotropic agent is organic bentonite.
[0075]The curing agent is an organic acid curing agent.
[0076] The film-forming catalyst is lanthanum oxide.
[0077] The epoxy equivalent of the epoxy resin is 3000-4500g / eq.
[0078] The amine resin is bismaleimide resin.
Embodiment 3
[0080] An environmentally friendly marine anti-corrosion coating suitable for large ships, consisting of the following components by weight percentage:
[0081] Epoxy 15%
[0082] Ultrafine Barium Sulfate 8%
[0083] Light Calcium Carbonate 8%
[0084] Thixotropic agent 3%
[0085] Curing agent 5%
[0086] Film-forming catalyst 0.2%
[0087] Algaecide 1%
[0088] Dispersant 2%
[0089] Amine resin 25
[0090] Nano silica 0.1%
[0091] Toner 5%
[0092] Silica powder balance.
[0093] The particle diameter of the silicon micropowder is 800 mesh, the particle diameter of the ultrafine barium sulfate is 500 mesh, and the nano silicon dioxide.
[0094] The thixotropic agent is organic bentonite.
[0095] The curing agent is an organic acid curing agent.
[0096] The film-forming catalyst is lanthanum oxide.
[0097] The epoxy equivalent of the epoxy resin is 3000-4500g / eq.
[0098] The amine resin is bismaleimide resin.
PUM
Property | Measurement | Unit |
---|---|---|
particle size (mesh) | aaaaa | aaaaa |
particle size (mesh) | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com