Embodiment 1
[0034] Fluorescent White Wall Repair Aerosol
[0035] Raw materials: 12kg of acrylic acid modified resin, 8kg of fluorescent white pigment, 2.4kg of talcum powder, 0.5kg of white carbon black, 10kg of 95% ethanol, 1kg of propylene glycol, 0.5Kg of GPE20, 35.5Kg of deionized water, 0.1kg of essence, dimethyl Ether 30kg.
[0036] The preparation method is as follows:
[0037] (1) Pre-dispersion: Put 10kg of 95% ethanol into the batching tank, then put it into a stirring and dispersing machine with a power of 22-35KW and a frequency conversion of 0-3000 rpm, start stirring slowly, and put in accurate metering while stirring Mix 8kg of fluorescent white pigment, 2.4kg of talcum powder and 0.5kg of white carbon black to obtain a thick color paste, which can be used for subsequent grinding.
[0038] (2) Grinding and dispersing: The pre-dispersed color paste is dispersed through colloid mill equipment, and the dispersed material liquid is filtered through a 100-mesh filter bag, whi...
Embodiment 2
[0042] Pearlescent White Interior Wall Repair Aerosol
[0043] Raw materials: 15kg of polyurethane resin, 8kg of 95% ethanol, 6kg of sparkling pearls, 0.4kg of white carbon black, 0.5kg of polyether modified silicon defoamer, 45kg of deionized water, 0.1kg of essence, and 25kg of dimethyl ether.
[0044] The preparation method is as follows:
[0045] (1) Preparation of agent solution: add 45kg of deionized water into the preparation pot, start stirring, slowly add 15kg of polyurethane resin, 8kg of 95% ethanol, 6kg of flashing pearl powder, 0.4kg of white carbon black, 0.5kg of polyether modified Materials such as non-toxic silicon defoamer, after basic mixing, disperse and stir at high speed for 30 minutes, then add 0.1kg of essence, stir for 5 minutes, and disperse evenly to obtain the dosage material.
[0046] (2) Filled tank finished product: with embodiment 1.
Embodiment 3
[0048] White interior wall repair aerosol
[0049] Raw materials: 13kg alkyd resin, 8kg 95% ethanol, 0.5kg white oil, 6kg titanium dioxide, 1.5kg bentonite, 0.4kg zinc stearate, 0.5kg silicone defoamer, 42kg deionized water, 0.1kg essence, di 28kg of methyl ether.
[0050] The preparation method is as follows:
[0051] (1) Preparation of agent solution: Add 42kg of deionized water into the preparation pot, start stirring, slowly add while stirring: 13kg of alkyd resin, 8kg of 95% ethanol, 0.5kg of white oil, 6kg of titanium dioxide, 1.5kg of bentonite, stearin Zinc acid 0.4kg, organosilicon defoamer 0.5kg and other materials, after basically mixing, disperse and stir at high speed for 30 minutes, then add 0.1kg essence, stir for 5 minutes, and disperse evenly to obtain the dosage material.
[0052] (2) Filled tank finished product: with embodiment 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com