Anti-fogging film
An anti-fog film and anti-fog coating technology, which is applied in application, coating, ink, etc., can solve the problems of affecting the normal growth of plants, reducing the light level in the shed, manpower and economic losses, etc., and achieves good low-temperature anti-fog performance , Improve the combination fastness, the effect of a wide range of use
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] A kind of anti-fog film, this anti-fog film comprises modified PET substrate layer and the anti-fog coating that is coated on the substrate layer; By weight, in described anti-fog coating, comprise: 50 parts of acrylic acid, 20 parts Parts of carbamate, 5 parts of lithium bromide, 2 parts of glycerin and 1 part of microcrystalline wax / montan wax dispersant; the modified PET substrate layer includes: 100 parts of polydipropyl terephthalate, 12 parts of glycerin Formate, 8 parts phosphite and 1 part silica. The preparation method of this anti-fog film, comprises the steps:
[0024] (1) Substrate ingredients: Weigh and mix the raw materials of the modified PET substrate layer in proportion, stir at high speed for 30 minutes at a stirring speed of 700-800 rpm, mix evenly, and set aside;
[0025] (2) Blown film: put the uniformly mixed substrate ingredients into the blown film machine, and obtain the modified PET film after extrusion, inflation molding, cooling and other st...
Embodiment 2
[0032] A kind of anti-fog film, this anti-fog film comprises modified PET substrate layer and the anti-fog coating that is coated on the substrate layer; By weight, described anti-fog coating comprises: 40 parts of acrylic acid, 15 parts Part urethane, 3 parts lithium bromide, 2 parts ethylene glycol and 1 part microcrystalline wax / montan wax dispersant; the modified PET substrate layer includes: 120 parts polydipropyl terephthalate, 10 parts Glyceryl formate, 10 parts phosphite and 1 part silica. The preparation method of this anti-fog film, comprises the steps:
[0033] (1) Substrate ingredients: Weigh and mix the raw materials of the modified PET substrate layer in proportion, stir at high speed for 30 minutes at a stirring speed of 700-800 rpm, mix evenly, and set aside;
[0034] (2) Blown film: put the uniformly mixed substrate ingredients into the blown film machine, and obtain the modified PET film after extrusion, inflation molding, cooling and other steps by flat ext...
PUM
| Property | Measurement | Unit |
|---|---|---|
| Thickness | aaaaa | aaaaa |
| Thickness | aaaaa | aaaaa |