Paint remover emulsion and preparation method thereof
A paint stripper and emulsion technology, applied in the field of paint stripper emulsion preparation, can solve problems such as paint stripper failure, surfactant failure, emulsion oil-water phase separation, etc., to reduce production costs, improve greening, and stabilize emulsions Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] 0.15% nano-SiO 2 (DEGUSSA hydrophilic silica A380), 0.05% of surfactant SDS and 0.15% of polymer PVP are placed in 47.65% of water, and 2% of methanol is added at the same time, stirred at 1000r.m.p for 24h, dubbed The aqueous phase of the lacquer. Prepare organic solvents such as 25% dichloromethane, 5% benzyl alcohol, 5% propiophenone, 5% formic acid, 5% oleic acid, and 5% anisole in proportion, put them in a beaker and ultrasonically for 20 minutes to fully mix all the solvents . The prepared oil phase was placed under a mechanical stirrer with a stirring speed of 1000 r.m.p. Then, slowly drop the prepared water phase into the oil phase, and stir for 30 minutes to prepare a paint remover emulsion. Finally, add a thickener to the prepared paint remover emulsion, and stir for 10 minutes at a stirring speed of 1000 r.m.p to prepare a paint remover with good stability. The prepared paint remover emulsion is placed at room temperature, and phase separation does not oc...
Embodiment 2
[0032] 0.2% nano-SiO 2 , 0.1% surfactant SDS and 0.5% polymer PVP are placed in 46.2% water, and 3% isopropanol is added at the same time, stirred at 1000r.m.p for 24h to form the aqueous phase of the paint remover. 20% of the organic solvent dichloromethane, 5% of 1,2-dichloroethane, 5% of benzyl alcohol, 5% of acetone, 10% of formic acid, 5% of phenetyl ether were prepared according to the proportion, and placed in a beaker for 30min sonication. All solvents are mixed thoroughly. The prepared oil phase was placed under a mechanical stirrer with a stirring speed of 800r.m.p. Then, slowly drop the prepared water phase into the oil phase, and stir for 30 minutes to prepare a paint remover emulsion. Finally, add a thickener to the prepared paint remover emulsion, and stir for 10 minutes at a stirring speed of 800 r.m.p to prepare a paint remover with good stability. The prepared paint remover emulsion is placed at room temperature, and phase separation does not occur after on...
Embodiment 3
[0034] 0.3% nano-SiO 2 , 0.15% surfactant CTAB and 1% polymer PVP are placed in 45.55% water, and 1.5% methanol and 1.5% isopropanol are added at the same time, stirred at 1000r.m.p for 24h to form the aqueous phase of the paint remover. Prepare organic solvents such as 20% dichloromethane, 5% 1,2-dichloroethane, 5% benzyl alcohol, 5% pentanone, 10% benzoic acid, and 5% phenetole, and place them in a beaker for 30 minutes of ultrasonication , so that all solvents are thoroughly mixed. The prepared oil phase was placed under a mechanical stirrer at a stirring speed of 1200 r.m.p. Then, slowly drop the prepared water phase into the oil phase, and stir for 30 minutes to prepare a paint remover emulsion. Finally, add a thickener to the prepared paint remover emulsion, and stir for 10 minutes at a stirring speed of 1200 r.m.p to prepare a paint remover with good stability. The prepared paint remover emulsion is placed at room temperature, and phase separation does not occur afte...