Method for modifying waste rubber-adhesive powder and producing composite rubber waterproof curling material

A composite rubber and waterproof membrane technology, applied in chemical instruments and methods, and other chemical processes, can solve problems such as poor physical properties such as strength, elongation, and dynamic performance, a large amount of waste gas, waste water, and high energy consumption in production processes. Achieve the effects of good dynamic performance, energy saving and performance improvement

Inactive Publication Date: 2007-11-21
天津市腾祥科技发展有限公司
View PDF0 Cites 15 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] Although the method of making reclaimed rubber from waste rubber comprehensively utilizes waste rubber, a large amount of waste gas and waste water are generated during the desulfurization process, which causes certain pollution to the surrounding ecological environment; moreover, the production process consumes a lot of energy. , the added value of the product is low; Among them, the regenerative softener that needs to be added in the dynamic desulfurization process mostly uses coal tar that is harmful to human health
[0005] At the same time, products made of reclaimed rubber have poor physical properties such as strength, elongation and dynamic properties.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0062] 1. Preparation of finely modified rubber powder

[0063] 1. Make fine rubber powder

[0064] After the waste tires are crushed, impurities are removed, and the part ≥ 40 mesh is fine rubber powder.

[0065] 2. Make fine mixed rubber powder

[0066] With fine rubber powder as the base amount, the ingredients are formulated according to the following weight ratio:

[0067] Fine rubber powder 100

[0068] Plasticizer - naphthenic oil 10

[0069] Modifier - polyalkylphenol disulfide 1

[0070] Mix the above components evenly to get fine mixed rubber powder.

[0071] 3. Preparation of finely modified rubber powder:

[0072] The finely mixed rubber powder is modified in a high-shear device at a temperature of 120±5°C.

[0073] When its performance reaches tensile strength ≥ 15Mpa, elongation at break ≥ 500%, it is finely modified rubber powder.

[0074] 2. Preparation of composite rubber waterproof membrane

[0075] 1. Preparation of Unvulcanized Vulcanized Films

...

Embodiment 2

[0108] 1. Preparation of finely modified rubber powder

[0109] 1. Make fine rubber powder

[0110] With embodiment 1.

[0111] 2. Make fine mixed rubber powder

[0112] With fine rubber powder as the base amount, the ingredients are formulated according to the following weight ratio:

[0113] Fine rubber powder 100

[0114] Plasticizer - naphthenic oil 12

[0115] Modifier - polyalkylphenol disulfide 0.8

[0116] Mix the above components evenly to get fine mixed rubber powder.

[0117] 3. Preparation of finely modified rubber powder:

[0118] With embodiment 1.

[0119] 2. Preparation of composite rubber waterproof membrane

[0120] 1 Preparation of unvulcanized vulcanized rubber sheet

[0121] Based on EPDM rubber, mix according to the following weight ratio

[0122] EPDM: 100

[0123] Fine modified rubber powder: 25

[0124] Accessories:

[0125] Active Agent - Zinc Oxide 5

[0126] Accelerator-M 1

[0127] Accelerator-TT 1.5

[0128] Vulcanizing agent - sul...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Tensile strengthaaaaaaaaaa
Tensile strengthaaaaaaaaaa
Heat resistanceaaaaaaaaaa
Login to View More

Abstract

The invention is concerned with waste rubber-rubber powder modifying, complex rubber waterproof rolled sheet made by the modified waste rubber-rubber powder and method. It is a comprehensive using for waste and old rubber. Step A is refining the modified rubber powder. Crush the waste and old rubber goods, remove impurity and take the part with over and equal to 40 mesh as fine rubber powder, then mix 100 fine rubber powder, 8 to 12 plasticizer and 0.5 to 1 modifier into fine mixing rubber powder, and modify the fine mixing rubber powder into highly shearing machine with 120+-5 degree. Step B is preparing the vulcanization rubber piece. The stuff is 100 synthetic rubber, 25 to 50 fine modified rubber powder, 2 to 8 zinc oxide, 0.5 to 2 accelerant M, 0.5 to 1.5 accelerant TT, 1 to 3 sulfur, 20 to 40 naphthene oil, 1 to 2 antioxidant A, 20 to 60 calcium carbonate, 40 to 80 carbon black. Mix and refine the synthetic rubber and fine modified rubber powder with the said stuff, except sulfidizing agent and accelerant. Add sulfidizing agent and accelerant with 80 to 90 degree and stop for 24 hours, and after refining again to get the molding piece. Step C is the production of un-vulcanization rubber piece. Mix and refine 100 butyl rubber, 8 to 10 polyisobutylene, 5 to 12 phenolic resin, 3 to 6 petroleum resin, 2 to 5 sodium oleate, 60 to 80 calcium carbonate and at 60 to 70 degree refine the mixture for 20 minutes again, then press or extrude the piece. Step D is complex vulcanization. Carry complex vulcanization on drum vulcanization machine to the vulcanization rubber piece without vulcanization and un-vulcanization rubber piece under the condition of 6 to 8 Mpa press to get the complex rubber waterproof rolled sheet. It uses for the waterproof layer to the underground building with high intention and extending nature, good dynamic capability.

Description

Technical field: [0001] The invention relates to a method for comprehensive utilization of waste rubber. In particular, it is a method for modifying waste rubber-rubber powder and using it to prepare composite rubber waterproof coiled material. Background technique: [0002] Waste rubber mainly comes from waste tires, waste rubber shoes, waste rubber hoses and scraps in the rubber production process. It belongs to industrial solid waste. In order to protect the living environment of human beings and develop a circular economy, the resource recycling and reuse of waste rubber , has drawn attention at home and abroad. [0003] At present, the comprehensive utilization of waste rubber is mainly to produce reclaimed rubber. For the production of reclaimed rubber from waste rubber, the method used is mainly the oil method; that is, at a temperature of 160-170 ° C, the waste rubber powder is processed through 6-8 After 1 hour of desulfurization process, it becomes reclaimed rubb...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): B29C43/24B29C47/12B29C35/04C08L9/00C08K5/372C09K3/18B29L9/00B29C48/30
Inventor 郑宏祥张子宏刘新酉杨涵于越
Owner 天津市腾祥科技发展有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products