Easily scrubbed graffiti art watercolor paint and preparation method

An art pigment and manufacturing method technology, applied in the field of painting supplies, can solve the problems of strong adhesion, difficult to scrub, difficult to dissolve, etc., and achieve the effects of film-forming, bright color, and prolonged shelf life

Inactive Publication Date: 2010-09-29
宋健
View PDF2 Cites 9 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

It is a pity that some art paints, such as traditional watercolors and gouache paints, are relatively easy to scrub with water, but due to their permeability, it is easy to leave difficult-to-clean colors on the walls and light-colored furniture surfaces; Such as acrylic paint, it is difficult to dissolve in water after drying and has strong adhesion and is difficult to scrub
These flaws make it difficult for people to accept graffiti art

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0029] Embodiment one: a kind of easy-to-clean watercolor graffiti art paint of the present invention comprises following components: its formula ratio is by weight parts:

[0030] 8 parts of low degree of alcoholysis polyvinyl alcohol

[0031] Modified ethylene oxide polyurethane emulsion 5 parts

[0032] Calcium carbonate 10 parts

[0033] Phthalocyanine green (pigment powder) 8 parts

[0034] 2 parts glycerin

[0035] Sodium benzoate 0.5 parts

[0036] Ethylparaben 0.05 parts

[0037] 30 parts of deionized water

[0038] A kind of manufacture method of the easy-to-clean watercolor graffiti art pigment of the present invention adopts the following process steps: its formula ratio is calculated in parts by weight:

[0039] 1. First heat 30 parts of deionized water, boil for 10 minutes to kill microorganisms, stop heating, add 0.05 parts of ethylparaben, 0.5 parts of sodium benzoate, and 2 parts of glycerin, and stir to dissolve.

[0040] 2. Add 8 parts of polyvinyl alc...

Embodiment 2

[0045] Embodiment two: a kind of easy-to-clean watercolor graffiti art paint of the present invention comprises following components: its formula ratio is by weight parts:

[0046] 18 parts of low alcoholysis polyvinyl alcohol

[0047] Modified ethylene oxide polyurethane emulsion 1 part

[0048] Calcium carbonate 5 parts

[0049] Iron oxide red (pigment powder) 22 parts

[0050] Iron oxide yellow (pigment powder) 3 parts

[0051] Glycerin 6 parts

[0052] Sodium benzoate 0.1 parts

[0053] Ethylparaben 0.3 parts

[0054] 45 parts deionized water

[0055] A kind of manufacture method of the easy-to-clean watercolor graffiti art pigment of the present invention adopts the following process steps: its formula ratio is calculated in parts by weight:

[0056] 1. First heat 45 parts of deionized water, boil for 10 minutes to kill microorganisms, stop heating, add 0.3 parts of ethylparaben, 0.1 parts of sodium benzoate, and 6 parts of glycerin, and stir to dissolve.

[0057] 2...

Embodiment 3

[0062] Embodiment three: a kind of easy-to-clean watercolor graffiti art paint of the present invention comprises the following components: its formula ratio is by weight:

[0063] 15 parts of low alcoholysis polyvinyl alcohol

[0064] Modified ethylene oxide polyurethane emulsion 3.5 parts

[0065] Calcium carbonate 8 parts

[0066] Ultramarine (pigment powder) 12 parts

[0067] 4 parts glycerin

[0068] Sodium benzoate 0.3 parts

[0069] Ethylparaben 0.15 parts

[0070] 40 parts deionized water

[0071] A kind of manufacture method of the easy-to-clean watercolor graffiti art paint of the present invention adopts following process steps:

[0072] 1. First heat 40 parts of deionized water, boil for 10 minutes to kill microorganisms, stop heating, add 0.15 parts of ethylparaben, 0.3 parts of sodium benzoate, and 4 parts of glycerin, and stir to dissolve.

[0073] 2. Add 15 parts of polyvinyl alcohol with low degree of alcoholysis and stir to completely dissolve into a m...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to an easily scrubbed graffiti art watercolor paint and a preparation method. The preparation method comprises the following steps of: heating and boiling deionized water to kill microorganism, then stopping heating, adding ethylparaben, sodium benzoate and glycerol, and stirring to dissolve the mixture; adding polyvinyl alcohol with low degree of alcoholysis, stirring to dissolve the mixture, then adding a modified ethylene oxide polyurethane emulsion, uniformly stirring the mixed solution to obtain the viscose, adding calcium carbonate and pigment powder into the viscose, and uniformly stirring the mixed solution to obtain the crude slurry; and adding the crude slurry into a hopper of a three-roll grinder, and allowing the crude slurry to flow into a grinding roller for grinding to obtain the color pigment slurry, and allowing the color pigment slurry to flow into a storage barrel to obtain the finished product. The easily scrubbed graffiti art watercolor paint has bright color and film-forming property, is difficult to permeate from the surface, and is easy to be scrubbed by cold and hot water; in addition, compared with the traditional paint which uses the sugar-derived material, such as water soluble starch, Arabic gum, peach gum and the like, the easily scrubbed graffiti art watercolor paint has the advantages that: according to the formula, non-sugar-derived material, namely polyvinyl alcohol with the low degree of alcoholysis is used, and the paint is more difficult to be utilized by the microorganism, such as mycete and the like, and the shelf life of the paint is obviously prolonged.

Description

technical field [0001] The invention relates to an easy-to-clean watercolor graffiti art paint and a manufacturing method, specifically belonging to the technical field of painting supplies. Background technique [0002] With social progress and economic development, young people like to express graffiti on glass doors, windows, interior walls and furniture on important anniversaries and eastern and western holidays with colorful and lively art paints in order to add joyful atmosphere or publicize their individuality. Art, draw comics and write auspicious blessings. It is a pity that some art paints, such as traditional watercolors and gouache paints, are relatively easy to scrub with water, but due to their permeability, it is easy to leave difficult-to-clean colors on the walls and light-colored furniture surfaces; Such as acrylic paint, it is difficult to dissolve in water after drying and has strong adhesion and is difficult to scrub. These defects make it difficult fo...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C09D5/06C09D129/04C09D175/04C09D7/12
Inventor 宋健
Owner 宋健
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products