Method for producing dry type duplicating body paper

A production method and technology for base paper, applied in papermaking, paper coatings, textiles and papermaking, etc., can solve the problems of affecting the qualified product rate, coating peeling, unreasonable selection ratio of fillers, etc., so as to improve the qualified product rate and control the production cost. , the effect of increasing the opacity

Inactive Publication Date: 2013-05-15
ZHENJIANG DADONG PULP & PAPER
View PDF3 Cites 13 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] In the traditional methods mentioned above, titanium dioxide and calcium carbonate are usually selected as fillers, and fillers are generally added during the pulping or sizing process. In this method, more fillers are lost during the dehydration process, and titanium dioxide is expensive, and the use of traditional processes will cause paper production costs. In addition, due to the unreasonable selection ratio of fillers and the loss of fillers will reduce the opacity of the dry copy paper, it is difficult to meet the higher requirements for use; in addition, the back of the dry copy paper needs to be coated, so for There are strict requirements on the coating absorption and wet deformation of base paper. The actual production effect of adding internal sizing agent in the traditional method is not good, and it is easy to cause wrinkles, unevenness, and peeling off of the colored coating on the back of the dry copy paper. Seriously affect the improvement of qualified product rate

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

example 1

[0018] Example 1: Papermaking weight is 50 g / m2

[0019] 1. Pulping: add 80% bleached chemical hardwood pulp and 20% bleached chemical softwood pulp to the pulper; then add titanium dioxide to mix with the evacuated wood pulp, the addition amount is 30 kg / ton of paper.

[0020] 2. Refining: Refining freeness is controlled at 380ml.

[0021] 3. Pulp preparation: add calcium carbonate, the addition amount is 180 kg / ton of paper.

[0022] 4. Sizing: add alkyl ketene dimer and polyamide epoxy resin to different positions, the addition amount of alkyl ketene dimer is 1.0 kg / ton of paper, and the amount of polyamide epoxy resin is 0.5 kg / ton Paper.

[0023] 5. After the pulp is dehydrated and pre-dried, tapioca oxidized starch and polyvinyl alcohol are added to the application formula of the surface sizing part. The mass ratio of tapioca oxidized starch and polyvinyl alcohol in the formula is 95:5, and the surface sizing part is absolutely dry The amount of substance added was 60...

example 2

[0025] Example 2: Papermaking weight is 40 g / m2

[0026] 1. Pulping: add 70% bleached chemical hardwood pulp and 30% bleached chemical softwood pulp to the pulper; then add titanium dioxide and mix with the evacuated wood pulp, the addition amount is 45 kg / ton paper. .

[0027] 2. Refining: Refining freeness is controlled at 420ml.

[0028] 3. Pulp preparation: add calcium carbonate, the amount added is 220 kg / ton of paper.

[0029] 4. Sizing: add alkyl ketene dimer and polyamide epoxy resin to different positions, the addition amount of alkyl ketene dimer is 1.5 kg / ton of paper, and the amount of polyamide epoxy resin is 1.0 kg / ton Paper.

[0030] 5. After the pulp is dehydrated and pre-dried, tapioca oxidized starch and polyvinyl alcohol are added to the application formula of the surface sizing part. The mass ratio of tapioca oxidized starch and polyvinyl alcohol in the formula is 95:5, and the surface sizing part is absolutely dry The amount of substance added was 40 k...

example 3

[0032] Example 3: Papermaking quantitative is 45g / m2

[0033] 1. Pulping: add 85% bleached chemical hardwood pulp and 15% bleached chemical softwood pulp to the pulper; then add titanium dioxide and mix with the evacuated wood pulp, the addition amount is 40 kg / ton paper.

[0034] 2. Refining: Refining freeness is controlled at 400ml.

[0035] 3. Pulp preparation: add calcium carbonate, the addition amount is 200 kg / ton of paper.

[0036]4. Sizing: add alkyl ketene dimer and polyamide epoxy resin to different positions, the addition amount of alkyl ketene dimer is 1.5 kg / ton of paper, and the amount of polyamide epoxy resin is 1.0 kg / ton Paper.

[0037] 5. After the pulp is dehydrated and pre-dried, tapioca oxidized starch and polyvinyl alcohol are added to the application formula of the surface sizing part. The mass ratio of tapioca oxidized starch and polyvinyl alcohol in the formula is 95:5, and the surface sizing part is absolutely dry The amount of substance added was ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
opacityaaaaaaaaaa
Login to view more

Abstract

The invention belongs to a papermaking technology, and relates to a method for producing dry type duplicating body paper. The method comprises the following steps of: making finished paper by crushing, grinding and mixing basic raw materials of bleached chemical broad-leaved wood pulp and bleached chemical softwood pulp, sizing, dehydrating, pre-drying, performing surface sizing, post-drying, glossing and coiling; during manufacturing, adding fillers, an inner sizing agent, a wet-strength agent and a surface sizing agent, wherein the two basic raw materials comprise 65-85 percent of bleached chemical broad-leaved wood pulp and 15-35 percent of bleached chemical softwood pulp, and the fillers comprise titanium dioxide and calcium carbonate; adding the titanium dioxide during pulp crushing, wherein the adding amount is 20-60 kilograms for per ton of paper; and adding the calcium carbonate during pulp mixing, wherein the adding amount is 120-280 kilograms for per ton of paper. With the method, the production cost can be reduced, the yield is improved, and the non transparency of a product is improved.

Description

technical field [0001] The invention belongs to papermaking technology, and relates to a production method of dry copying base paper. Background technique [0002] The existing dry copy base paper production method is that the mixed wood pulp basic raw material of bleached chemical hardwood pulp and bleached chemical softwood pulp is pulped, refined, blended, sized, dehydrated, pre-dried, surface sizing, After drying, calendering, coiling and other processes to make paper, fillers, internal sizing agents, wetting strength agents, surface sizing agents and other additives are added in the manufacturing process. [0003] In the traditional methods mentioned above, titanium dioxide and calcium carbonate are usually selected as fillers, and fillers are generally added during the pulping or sizing process. In this method, more fillers are lost during the dehydration process, and titanium dioxide is expensive, and the use of traditional processes will cause paper production costs....

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): D21H11/00D21H17/67D21H21/16D21H21/20D21H19/14D21H19/20
Inventor 陈袁星陈国平戴罗根谭宁华蔡兆斌
Owner ZHENJIANG DADONG PULP & PAPER
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products