Embodiment 1
[0032] Preparation of modified nano-zinc powder:
[0033]
[0034] According to the above mass percentage, tert-butyl mercaptan, octadecyl mercaptan, octadecyl dimethyl benzyl ammonium chloride, dodecyl trimethyl ammonium chloride, 4-hydroxybenzotrimethyl ammonium Azole, benzotriazole, disodium ethylenediaminetetraacetic acid and sodium tartrate were added to deionized water, under the action of ultrasonic dispersion with a frequency of 24kHz and a power of 3kW, stirring for 0.4h, and then adding nanometer zinc powder, Further, under the action of ultrasonic dispersion with a frequency of 24kHz and a power of 3kW, it was stirred for 4.5h, and then the modified nano-zinc powder was obtained through centrifugation, deionized water washing, centrifugation, vacuum drying, grinding and sieving. The modified nano-zinc powder is ready for use;
[0035] Preparation of lubricating oil with modified nano-zinc powder and ionic liquid:
[0036]
[0037]
[0038] According to th...
Embodiment 2
[0040] Preparation of modified nano-zinc powder:
[0041]
[0042] According to the above mass percentage, n-butyl mercaptan, phenethyl mercaptan, dodecyltrimethylammonium bromide, tetradecyldimethylpyridinium bromide, hexadecyldimethylbenzyl Ammonium bromide, methyl benzotriazole, sodium citrate and potassium tartrate were added into deionized water, under the action of ultrasonic dispersion with a frequency of 28kHz and a power of 5kW, after stirring for 0.4h, nanometer zinc powder was added, further Under the action of ultrasonic dispersion with a frequency of 28kHz and a power of 5kW, stir for 3.0h, then undergo centrifugation, deionized water washing, centrifugation, vacuum drying, grinding and sieving to obtain modified nano-zinc powder. Modified nano-zinc powder for standby;
[0043] Preparation of lubricating oil with modified nano-zinc powder and ionic liquid:
[0044]
[0045] According to the above mass percentages, 1-methyl-3-butylimidazolium tetrafluorobor...
Embodiment 3
[0047] Preparation of modified nano-zinc powder:
[0048]
[0049] According to the above mass percentage, n-dodecyl mercaptan, n-pentyl mercaptan, dodecyl dimethyl benzyl ammonium chloride, octadecyl trimethyl ammonium bromide, N-hydroxybenzo Add triazole, benzotriazole, edetate disodium salt and potassium citrate into deionized water, stir for 0.3h under ultrasonic dispersion with a frequency of 38kHz and a power of 8kW, and then add nano-zinc Powder, further under the action of ultrasonic dispersion with a frequency of 38kHz and a power of 8kW, stirred for 2.5h, then centrifuged, washed with deionized water, centrifuged, vacuum dried, ground and sieved to obtain modified nano-zinc powder, The prepared modified nano-zinc powder is standby;
[0050] Preparation of lubricating oil with modified nano-zinc powder and ionic liquid:
[0051]
[0052] According to the above mass percentage, N-butylpyridinium hexafluorophosphate, modified nano-zinc powder, calcium alkyl sali...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com