Unlock instant, AI-driven research and patent intelligence for your innovation.

Preparation method for pyrolysis-oxidized starchiness cigarette humectant and application thereof

A humectant and oxidized starch technology for tobacco, which is applied in the field of cigarettes, can solve the problems of high cost, few sources of raw materials, and complicated preparation process, and achieve the effects of improving processing resistance, reducing tobacco leaf consumption, and having a wide range of sources

Active Publication Date: 2015-04-22
ZHENGZHOU TOBACCO RES INST OF CNTC
View PDF2 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the above-mentioned natural plant extract moisturizers generally have problems such as complicated preparation process, high cost, and few sources of raw materials, so they have not been widely used.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Preparation method for pyrolysis-oxidized starchiness cigarette humectant and application thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0020] Example 1. Weigh 350g of corn starch, add 5g of 65% concentrated nitric acid dropwise, stir and mix evenly, put it into a self-made dry reactor, react at 120°C for 4 hours, and neutralize it with 10% sodium hydroxide ethanol aqueous solution after cooling , and then dried, crushed and sieved to obtain pyrolytic dextrin. Add pyrolytic dextrin to ethanol / water (V / V=60:40) solution to make 35% starch milk, then use 5% sodium hydroxide aqueous solution to adjust the pH value to 8-10, at 1-2 Add 20g sodium hypochlorite within 1 hour, and react at 50°C for 7 hours. During the reaction, continuously add 5% aqueous sodium hydroxide solution dropwise to stabilize the pH value at 8-10. After the reaction, use 20% hydrochloric acid ethanol / The aqueous solution is neutralized to neutral, and excess sodium hypochlorite is reduced with sodium sulfite, and finally dehydration, washing, drying, crushing and sieving are carried out respectively to obtain pyrolysis-oxidized starch. T...

Embodiment 2

[0021] Example 2. Weigh 350g of cornstarch, add 10g of 65% concentrated nitric acid dropwise, stir and mix evenly, put it into a self-made dry reactor, react at 130°C for 6 hours, cool it with 10% sodium hydroxide ethanol aqueous solution Neutralized, then dried, pulverized and sieved to obtain pyrolytic dextrin. Add pyrolytic dextrin to ethanol / water (V / V=60:40) solution to make 35% starch milk, then use 5% sodium hydroxide aqueous solution to adjust the pH value to 8-10, at 1-2 Add 22g of sodium hypochlorite within 1 hour, and react for 7 hours at 50°C. During the reaction, continuously add 5% aqueous sodium hydroxide solution dropwise to stabilize the pH value at 8-10. The aqueous solution is neutralized to neutral, and excess sodium hypochlorite is reduced with sodium sulfite, and finally dehydration, washing, drying, crushing and sieving are carried out respectively to obtain pyrolysis-oxidized starch. The pyrolyzed-oxidized starch is dissolved in water to form a 40% aq...

Embodiment 3

[0022] Example 3. Weigh 350g of barley starch, add 15g of concentrated sulfuric acid dropwise, stir and mix evenly, put it into a self-made dry reactor, react at 140°C for 8 hours, and neutralize it with 10% sodium hydroxide ethanol aqueous solution after cooling , and then dried, crushed and sieved to obtain pyrolytic dextrin. Add pyrolytic dextrin to ethanol / water (V / V=70:30) solution to make 35% starch milk, then use 5% sodium hydroxide aqueous solution to adjust the pH value to 8-10, at 1-2 Add 55g of sodium hypochlorite within 1 hour, and react at 50°C for 8 hours. During the reaction, continuously add 5% aqueous sodium hydroxide solution dropwise to stabilize the pH value at 8-10. After the reaction, use 20% hydrochloric acid ethanol / The aqueous solution is neutralized to neutral, and excess sodium hypochlorite is reduced with sodium sulfite, and finally dehydration, washing, drying, crushing and sieving are carried out respectively to obtain pyrolysis-oxidized starch....

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

Provided are a preparation method for a pyrolysis-oxidized starchiness cigarette humectant and application thereof. The preparation method is characterized in that the humectant is formed by pyrolysis and oxidation modification and formed by adding 2-20g of 65% concentrated nitric acid, 400-1200g of ethanol / aqueous solution and 5-60g of sodium hypochlorite to per 350g of starch. The preparation method has the advantages that the used raw material is the starch, and the starch belongs to renewable resources and is extensive in source and low in cost; by performing on pyrolysis modification and oxidation modification, the starch is high in water absorption and water retaining capability, green, environmentally friendly and low in cost. The humectant is evenly sprayed on tobaccos in a tobacco adding process, the tobacco processing durability can be improved, tobacco breaking in the processing process is reduced, tobacco consumption of cigarettes is reduced, the effects of improving taste and reducing flue gas stimulation can be achieved, and the effects of improving tobacco physical moisturizing and sense moisturizing are achieved simultaneously.

Description

technical field [0001] The invention belongs to the technical field of cigarettes, and specifically relates to a preparation method and application of a pyrolysis-oxidized starch-based humectant for tobacco. Moisturizing effect for the senses. Background technique [0002] Humectants are an indispensable additive in the production process of cigarettes. During the production, transportation, storage, sales and smoking of cigarettes, humectants can effectively maintain the moisture of tobacco leaves, increase the softness of tobacco leaves, and improve the durability of tobacco leaves. Processing performance, reduce the crushing of tobacco leaves during processing, and reduce the consumption of tobacco leaves in cigarettes. At the same time, the humectant also has the effect of reducing smoke irritation and improving taste and taste. [0003] At present, the humectants used by domestic cigarette manufacturers mainly include polyols such as propylene glycol, glycerin and sor...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): A24B15/40C08B31/18
Inventor 张晓兵刘惠民王宜鹏贾云祯彭斌
Owner ZHENGZHOU TOBACCO RES INST OF CNTC