Water type colorful coating
A multi-color paint, water-type technology, applied in the field of paint, can solve the problems of poor dispersibility, scrub resistance, friction resistance, etc., and achieve the effect of good dispersibility, good decorative effect and bright colors
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A kind of water-type colorful paint, its raw material ratio is as follows in parts by weight: 100 parts of hydroxyethyl cellulose; 15 parts of isopropanol; 20 parts of sodium hydroxide; 40 parts of xylene; 10 parts of sodium carboxymethyl cellulose ; 5 parts of lead naphthenate; 80 parts of deionized water; 15 parts of cobalt naphthenate; 10 parts of iron oxide green; 25 parts of modified bentonite; 20 parts of sodium polystyrene sulfonate; 10 parts of talcum powder; 4 parts of dibutyl formate; 30 parts of titanium dioxide; 10 parts of sodium naphthalenesulfonate; 20 parts of zinc phosphate.
[0016] Add hydroxyethyl cellulose, sodium hydroxide, xylene, sodium carboxymethyl cellulose and lead naphthenate to deionized water, heat to 40°C and stir for 3 hours, add cobalt naphthenate, modified bentonite, polystyrene Sodium sulfonate, talcum powder, sodium naphthalene sulfonate and dibutyl phthalate, heated up to 50°C and milled with a ball mill for 10 minutes, added isopro...
Embodiment 2
[0019] A kind of water-type colorful paint, its raw material ratio is as follows in parts by weight: 100 parts of hydroxyethyl cellulose; 25 parts of isopropanol; 30 parts of sodium hydroxide; 50 parts of xylene; 20 parts of sodium carboxymethyl cellulose ; 15 parts of lead naphthenate; 90 parts of deionized water; 35 parts of cobalt naphthenate; 20 parts of iron oxide red; 35 parts of modified bentonite; 40 parts of sodium polystyrene sulfonate; 30 parts of talcum powder; 10 parts of dibutyl formate; 40 parts of titanium dioxide; 20 parts of sodium naphthalenesulfonate; 30 parts of zinc phosphate.
[0020] Add hydroxyethyl cellulose, sodium hydroxide, xylene, sodium carboxymethyl cellulose and lead naphthenate to deionized water, heat to 40°C and stir for 3 hours, add cobalt naphthenate, modified bentonite, polystyrene Sodium sulfonate, talcum powder, sodium naphthalene sulfonate and dibutyl phthalate, heated up to 50°C and milled with a ball mill for 10 minutes, added isopro...
Embodiment 3
[0023] A kind of water-type colorful paint, its raw material ratio is as follows in parts by weight: 100 parts of hydroxyethyl cellulose; 20 parts of isopropanol; 25 parts of sodium hydroxide; 45 parts of xylene; 15 parts of sodium carboxymethyl cellulose ; 10 parts of lead naphthenate; 85 parts of deionized water; 25 parts of cobalt naphthenate; 15 parts of iron oxide yellow; 30 parts of modified bentonite; 30 parts of sodium polystyrene sulfonate; 20 parts of talcum powder; 7 parts of dibutyl formate; 35 parts of titanium dioxide; 15 parts of sodium naphthalenesulfonate; 25 parts of zinc phosphate.
[0024] Add hydroxyethyl cellulose, sodium hydroxide, xylene, sodium carboxymethyl cellulose and lead naphthenate to deionized water, heat to 40°C and stir for 3 hours, add cobalt naphthenate, modified bentonite, polystyrene Sodium sulfonate, talcum powder, sodium naphthalene sulfonate and dibutyl phthalate, heated up to 50°C and milled with a ball mill for 10 minutes, added isop...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com