Plugging agent used for drilling fluid and preparation method thereof
A plugging agent and drilling fluid technology, applied in the field of drilling, can solve the problems of poor plugging effect of mud shale and inability to ensure well wall stability, etc., achieve good plugging, reduce the occurrence of downhole complex situations, and reduce API fluid loss Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] Weigh raw materials: 200g of bentonite, 100g of acrylamide, 25g of 2-acrylamide-2-methylpropanesulfonic acid, 4g of sodium hydroxide, 100g of 1000 mesh calcium carbonate, 300g of water, N,N'-methylene Bisacrylamide 0.2g, sodium bisulfite 2g, ammonium persulfate 2g.
[0028] Preparation:
[0029] Step 1: adding the above-mentioned raw materials weighed into a kneader and stirring evenly to obtain a raw material mixture;
[0030] In the embodiment of the present invention, this step specifically includes:
[0031] 1a: Dissolve the weighed acrylamide and 2-acrylamido-2-methylpropanesulfonic acid into the weighed water, and then add them together into the kneader, and then add the weighed hydroxide Sodium, bentonite and 1000 mesh calcium carbonate, stir well;
[0032] Since bentonite can absorb acrylamide solution, dissolving acrylamide in water first and then mixing with other raw materials is more conducive to the uniform mixing of acrylamide and bentonite.
[0033] I...
Embodiment 2
[0040] Weigh raw materials: 180g of bentonite, 90g of acrylamide, 20g of 2-acrylamide-2-methylpropanesulfonic acid, 3g of potassium hydroxide, 90g of 1000 mesh calcium carbonate, 280g of water, N,N'-methylenebis Acrylamide 0.1g, sodium bisulfite 1.5g, ammonium persulfate 1.5g.
[0041] Preparation:
[0042] Step 1: same as embodiment one, only difference is that potassium hydroxide replaces sodium hydroxide;
[0043] Step 2: heating the above raw material mixture at 40°C and stirring for 0.5 hours to obtain a block jelly;
[0044] Step 3: Same as Embodiment 1.
Embodiment 3
[0046] Weigh raw materials: 220g of bentonite, 110g of acrylamide, 30g of 2-acrylamido-2-methylpropanesulfonic acid, 5g of sodium hydroxide, 110g of 1000 mesh calcium carbonate, 320g of water, N,N'-methylenebis Acrylamide 0.3g, sodium bisulfite 2.5g, ammonium persulfate 2.5g.
[0047] Preparation:
[0048] Step 1: same as embodiment one;
[0049] Step 2: heating the above raw material mixture at 60°C and stirring for 1 hour to obtain a block jelly;
[0050] Step 3: Same as Embodiment 1.