A kind of processing method of corrosion-resistant filler
A processing method and corrosion-resistant technology, applied in chemical instruments and methods, chemical/physical/physical-chemical processes, chemical/physical processes, etc., can solve the problems of corrosion and aging of fillers, complex components, etc., and achieve corrosion resistance and Increased strength, low energy consumption, and reduced energy consumption
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2017-07-04
Abstract
Description
technical field
[0001] The invention relates to a processing method for corrosion-resistant packing, which belongs to the technical field of petrochemical mass transfer and separation equipment. Background technique
[0002] In chemical engineering, packing refers to inert solid materials installed in packed towers, such as Pall rings and Raschig rings, etc., whose function is to increase the contact surface of gas-liquid and make them strongly mix with each other. Bulk packing is a granular body with a certain geometric shape and size, which is generally piled up in the tower in a random manner, also known as random packing or granular packing. According to different structural characteristics, bulk packing can be divided into ring packing, saddle packing, ring saddle packing and spherical packing.
[0003] At present, the packed tower has been widely used in unit operations such as rectification, absorption, extraction, etc. in chemical, petroleum, pharmaceutical, environ...
Examples
Embodiment
[0020] A kind of processing method of corrosion-resistant filler of the present embodiment, comprises the following steps:
[0021] (1) Ingredients: The parts by weight of each component in the raw material of the corrosion-resistant filler are: 4-5 parts of tungsten carbide, 2-3 parts of Zn, 7-8 parts of montmorillonite, 20-25 parts of kaolin, AlN powder 4-5 parts, 6-8 parts of wollastonite, 6-8 parts of diopside, 5-6 parts of antioxidant RD and 38-42 parts of clay;
[0022] (2) Grinding: Use a pulverizer to pulverize the above-mentioned raw materials respectively, and the particle diameter of the pulverized raw materials is between 15mm-18mm;
[0023] (3) Mixing ball milling: the raw materials are put into the mixing ball mill according to the parts by weight for mixing ball milling, and the particle diameter of the raw materials after the mixing ball milling is between 2000-4500 mesh;
[0024] (4) Adding water: adding water to the raw materials after mixing and ball millin...