Paper difficult to tear and preparation method thereof
A technology for paper and filter paper, applied in the field of paper preparation, can solve problems such as lack of environmental protection degradation function, and achieve the effects of low cost, high air permeability and opacity, and simple preparation process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] A hard-to-tear paper made from:
[0026] 30 parts of polylactic acid fiber, 20 parts of anionic starch, 20 parts of absolute ethanol, 20 parts of industrial filter paper, 40 parts of alkyl ketene dimer, 30 parts of solid paraffin, 20 parts of vinyltrimethoxysilane.
[0027] Its preparation method is:
[0028] Disperse polylactic acid fiber and anionic starch in absolute ethanol to make a 5% suspension, and vibrate ultrasonically for 15 minutes in an ultrasonic oscillator; cut industrial filter paper into small discs with a diameter of about 5 cm, and then put them in In the 5% filler anhydrous ethanol suspension, vertically pull it repeatedly 3 times, so that the solid filler particles are evenly distributed on the surface of the industrial filter paper to increase the surface roughness of the paper, air-dry naturally, and set aside, the industrial filter paper prepared above Put the sheet into a 15% ethanol solution of hydrophobic agent (alkyl ketene dimer (AKD), soli...
Embodiment 2
[0030] A hard-to-tear paper made from:
[0031] 35 parts of polylactic acid fiber, 25 parts of anionic starch, 25 parts of absolute ethanol, 25 parts of industrial filter paper, 45 parts of alkyl ketene dimer, 35 parts of solid paraffin, 25 parts of vinyltrimethoxysilane.
[0032] Its preparation method is:
[0033] Disperse polylactic acid fiber and anionic starch in absolute ethanol to make a 10% suspension, and ultrasonically vibrate in an ultrasonic oscillator for 20 minutes; cut industrial filter paper into small discs with a diameter of about 6 cm, and then put them in In the 5-25% filler anhydrous ethanol suspension, vertically pull it repeatedly 4 times, so that the solid filler particles are evenly distributed on the surface of the industrial filter paper to increase the surface roughness of the paper, air-dried naturally, and set aside. Put the industrial filter paper into 20% ethanol solution of hydrophobic agent (alkyl ketene dimer (AKD), solid paraffin, vinyltrim...
Embodiment 3
[0035] A hard-to-tear paper made from:
[0036] 40 parts of polylactic acid fiber, 30 parts of anionic starch, 30 parts of absolute ethanol, 30 parts of industrial filter paper, 50 parts of alkyl ketene dimer, 40 parts of solid paraffin, 30 parts of vinyltrimethoxysilane.
[0037] Its preparation method is:
[0038] Disperse polylactic acid fiber and anionic starch in absolute ethanol to make a 15% suspension, and ultrasonically vibrate in an ultrasonic oscillator for 25 minutes; cut industrial filter paper into small discs with a diameter of about 7cm, and then put them in In the 15% filler anhydrous ethanol suspension, vertically pull it repeatedly 5 times, so that the solid filler particles are evenly distributed on the surface of the industrial filter paper to increase the surface roughness of the paper, naturally air-dried, and set aside, the industrial filter paper prepared above Put the sheet into a 25% ethanol solution of hydrophobic agent (alkyl ketene dimer (AKD), s...
PUM