A method for preparing dissolving pulp from cotton linters
A technology of cotton linters and dissolving pulp, which is applied in pulping with inorganic alkali, pulping of cellulose raw materials, pulp bleaching, etc., can solve the problems of large pollution, harsh reaction conditions, and large amount of medicines, etc., to reduce production costs, The effect of reducing the degree of polymerization and reducing the amount of alkali used
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0019] A method for preparing dissolving pulp from cotton linters, comprising enzyme treatment, steam bleaching treatment and acid treatment, wherein sulfuric acid is firstly used for acid pretreatment before enzyme treatment.
[0020] The specific steps are:
[0021] Step 1: Acid Pretreatment
[0022] Add 1Kg (absolute dry weight) of cotton linters for raw materials in the stainless steel stirred tank, add sulfuric acid with a pH of 1.5, adjust the slurry concentration to 9%, and process at 30° C. for 12 hours.
[0023] Step 2: Enzyme Treatment
[0024] Wash the slurry after the acid treatment, after washing, add dipotassium hydrogen phosphate-potassium dihydrogen phosphate buffered saline solution to the system, adjust the pH of the system to 7.5, and the slurry concentration is 5%, add 150000U ferulic acid esterase, The ratio of lipase, ferulic acid esterase and lipase enzyme dosage is 8:3, and treated at 70° C. for 2 hours.
[0025] The third step: chemical steam bleach...
Embodiment 2
[0034] A method for preparing dissolving pulp from cotton linters, comprising enzyme treatment, steam bleaching treatment and acid treatment, wherein sulfuric acid is firstly used for acid pretreatment before enzyme treatment.
[0035] The specific steps are:
[0036] Step 1: Acid Pretreatment
[0037] Add 1Kg (absolute dry weight) of cotton linters for the preparation in the stainless steel stirred tank, add the sulfuric acid that pH is 4, adjust the slurry concentration to be 10%, and process at 90° C. for 2 hours.
[0038] Step 2: Enzyme Treatment
[0039] Wash the slurry after acid treatment. After washing, add dipotassium hydrogen phosphate-potassium dihydrogen phosphate buffered saline solution to the system to adjust the pH of the system to 6.5, and the slurry concentration is 6%. Add 15000U lipase and cellulase , the enzyme dosage ratio of lipase and cellulase was 4:15, and treated at 45°C for 35h.
[0040] The third step: chemical steam bleaching treatment
[0041...
Embodiment 3
[0049] A method for preparing dissolving pulp from cotton linters, comprising enzyme treatment, steam bleaching treatment and acid treatment, wherein sulfuric acid is firstly used for acid pretreatment before enzyme treatment.
[0050] The specific steps are:
[0051] Step 1: Acid Pretreatment
[0052] Add 1Kg (absolute dry weight) of cotton linters for raw materials into the stainless steel stirred tank, add sulfuric acid with a pH of 5, adjust the slurry concentration to 9%, and process at 70°C for 7 hours.
[0053] Step 2: Enzyme Treatment
[0054] Wash the slurry after the acid treatment. After washing, add dipotassium hydrogen phosphate-potassium dihydrogen phosphate buffered saline solution to adjust the pH of the system to 8, and the slurry concentration is 7%. Add 100000U ferulic acid esterase and The ratio of cellulase, ferulic acid esterase and cellulase is 9:23, and treated at 65°C for 10 hours.
[0055] The third step: chemical steam bleaching treatment
[0056...
PUM
| Property | Measurement | Unit |
|---|---|---|
| length | aaaaa | aaaaa |
| Ash content | aaaaa | aaaaa |
| Ash content | aaaaa | aaaaa |