Embodiment 1
[0026] An example of the sulfur-oxygen symbiosis mixed antimony ore flotation recovery method of the present invention comprises the following steps and medicament system:
[0027] 1. Mineral raw materials:
[0028] The material used is sulfur-oxygen symbiotic mixed antimony ore, and the antimony content in the ore is 1.59%. The phase analysis of antimony shows that the antimony minerals are mainly stibnite, and also contain some antimonite, stibnite and a small amount of stibnite. Among them, the proportion of stibnite is 74.24%, antimonite is 14.45%, stibnite is 5.11%, yellow antimonite is 2.65%, and other antimony minerals are 3.55%.
[0029] 2. Flotation agents and operating conditions:
[0030]
[0031] During the flotation process, the sulfur-oxygen symbiotic mixed antimony ore is ground until the mineral monomers are dissociated, and then sodium hexametaphosphate is added as a mineral dispersant, potassium permanganate is used as a mineral oxidant, sodium sulfide i...
Embodiment 2
[0033] Another example of the sulfur-oxygen symbiosis mixed antimony ore flotation recovery method of the present invention comprises the following steps and medicament system:
[0034] 1. Mineral raw materials:
[0035] The material used is sulfur-oxygen symbiotic mixed antimony ore, and the antimony content in the ore is 1.90%. The phase analysis of antimony shows that the antimony minerals are mainly stibnite, and also contain some antimonite, stibnite and a small amount of stibnite. Among them, the proportion of stibnite is 76.12%, antimonite is 13.50%, stibnite is 4.17%, yellow antimonite is 3.20%, and other antimony minerals are 3.01%.
[0036] 2. Flotation agents and operating conditions:
[0037]
[0038] During the flotation process, the sulfur-oxygen symbiotic mixed antimony ore is ground until the mineral monomers are dissociated, and then sodium hexametaphosphate is added as a mineral dispersant, potassium permanganate is used as a mineral oxidant, sodium sulf...
Embodiment 3
[0040] Another example of the sulfur-oxygen symbiosis mixed antimony ore flotation recovery method of the present invention comprises the following steps and medicament system:
[0041] 1. Mineral raw materials:
[0042] The material used is sulfur-oxygen symbiotic mixed antimony ore, and the antimony content in the ore is 2.56%. The phase analysis of antimony shows that the antimony minerals are mainly stibnite, and also contain some antimonite, stibnite and a small amount of stibnite. Among them, the proportion of stibnite is 78.66%, antimonite is 10.81%, stibnite is 6.55%, yellow antimonite is 2.49%, and other antimony minerals are 1.49%.
[0043] 2. Flotation agents and operating conditions:
[0044]
[0045] During the flotation process, the sulfur-oxygen symbiotic mixed antimony ore is ground until the mineral monomers are dissociated, and then sodium hexametaphosphate is added as a mineral dispersant, potassium permanganate is used as a mineral oxidant, sodium sulf...
PUM
Property | Measurement | Unit |
---|---|---|
recovery rate | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com