Heat resistant ultraviolet curable coating
A technology of curing coatings and ultraviolet light, which is applied in the direction of fire-resistant coatings and coatings, and can solve the problems of heat-resistant coatings fading, high volatile organic compound emissions, environmental friendliness and high efficiency.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] The present embodiment provides a kind of high temperature resistant ultraviolet light curing coating, and its composition comprises by weight:
[0029] 45 parts of maleated epoxy soybean oil acrylate;
[0030] 1.5 parts of photoinitiator;
[0031] 1 part of triethylamine;
[0032] Heat-resistant dosage 0.02 parts;
[0033] 35 parts of water;
[0034] 12 parts ethanol
[0035] The heat-resistant agent includes 2% acetaldehyde oxime, 3% chloral, 1% lithium phosphate and the balance of mannitol by mass.
[0036] Further, the photoinitiator is selected from 2-hydroxyl-2-methylpropiophenone.
[0037] Furthermore, its preparation method includes the following steps:
[0038] 1) preparing the maleated epoxy soybean oil acrylate;
[0039] 2) Add triethylamine to maleated epoxy soybean oil acrylate and stir, then add water, stir for 15 minutes, then add photoinitiator, heat resistant agent and ethanol and stir for 30 minutes.
[0040] The maleated epoxidized soybean oil...
Embodiment 2
[0043] The present embodiment provides a kind of high temperature resistant ultraviolet light curing coating, and its composition comprises by weight:
[0044] 60 parts of maleated epoxy soybean oil acrylate;
[0045] 1 part of photoinitiator;
[0046] 1.5 parts of triethylamine;
[0047] Heat-resistant dosage 0.01 part;
[0048] 40 parts of water;
[0049] 10 parts ethanol
[0050] The heat-resistant agent includes 2% acetaldehyde oxime, 3% chloral, 1% lithium phosphate and the balance of mannitol by mass.
[0051] Further, the photoinitiator is selected from 2-hydroxyl-2-methylpropiophenone.
[0052] Furthermore, its preparation method includes the following steps:
[0053] 1) preparing the maleated epoxy soybean oil acrylate;
[0054] 2) Add triethylamine to maleated epoxy soybean oil acrylate and stir, then add water, stir for 15 minutes, then add photoinitiator, heat resistant agent and ethanol and stir for 30 minutes.
[0055] This embodiment also includes defoam...
Embodiment 3
[0057] The present embodiment provides a kind of high temperature resistant ultraviolet light curing coating, and its composition comprises by weight:
[0058] 35 parts of maleated epoxy soybean oil acrylate;
[0059] 2.5 parts of photoinitiator;
[0060] 0.5 part of triethylamine;
[0061] Heat-resistant dosage 0.03 parts;
[0062] 20 parts of water;
[0063]15 parts ethanol
[0064] The heat-resistant agent includes 2% acetaldehyde oxime, 3% chloral, 1% lithium phosphate and the balance of mannitol by mass.
[0065] Further, the photoinitiator is selected from 2-hydroxyl-2-methylpropiophenone.
[0066] Furthermore, its preparation method includes the following steps:
[0067] 1) preparing the maleated epoxy soybean oil acrylate;
[0068] 2) Add triethylamine to maleated epoxy soybean oil acrylate and stir, then add water, stir for 15 minutes, then add photoinitiator, heat resistant agent and ethanol and stir for 30 minutes.