Magnetic wool fabric prepared by using inorganic sulfur-containing reductive agent
A technology of reducing agent and wool, which is applied in the field of using inorganic sulfur-containing reducing agent to prepare magnetic wool fabric, which can solve the problems of difficult control, long process, low washing fastness, etc., and achieve the effect of reducing damage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0013] (1) Dissolve 3.5g of sodium sulfide, 40g of urea and 3g of sodium lauryl sulfate into water to form a 100g mixed solution, then add 0.3g of magnetic nano-particle nickel ferrite, and stir vigorously to prepare a dispersed magnetic nano-particle nickel Ferrite solution;
[0014] (2) padding the woolen fabric in the solution solution obtained in step (1) several times, and the excess rate is 80%;
[0015] (3) Heat the padded wool fabric under hot air at 120°C for 15 minutes;
[0016] (4) Soak the heated wool fabric in saturated sodium chloride aqueous solution for 10 minutes, then wash and dry.
Embodiment 2
[0018] (1) Dissolve 4g of sodium metabisulfite, 30g of urea and 4g of sodium lauryl sulfate into water to form a 100g mixed solution, then add 0.8g of magnetic nanoparticle cobalt ferrite, and stir vigorously to prepare cobalt iron with magnetic nanoparticles dispersed Oxygen solution;
[0019] (2) padding the woolen fabric in the solution solution obtained in step (1) several times, and the excess rate is 100%;
[0020] (3) Heat the padded wool fabric under hot air at 120°C for 15 minutes;
[0021] (4) Soak the heated wool fabric in saturated sodium chloride aqueous solution for 10 minutes, then wash and dry.
Embodiment 3
[0023] (1) Dissolve 5g of sodium bisulfite, 50g of urea and 2g of sodium lauryl sulfate into water to form a 100g mixed solution, then add 1.2g of magnetic nanoparticle magnesium ferrite, and stir vigorously to prepare dispersed magnetic nanoparticles Dissolving solution of magnesium ferrite;
[0024] (2) padding the woolen fabric in the solution solution obtained in step (1) several times, and the excess rate is 90%;
[0025] (3) Heat the padded wool fabric under hot air at 80°C for 30 minutes;
[0026] (4) Soak the heated wool fabric in saturated sodium chloride aqueous solution for 10 minutes, then wash and dry.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com