A kind of vest bag dispensing glue and preparation method thereof
A vest bag and glue dispensing technology is applied in the directions of adhesives, rosin adhesives, adhesive additives, etc., which can solve the problems of high glue cost, long curing time, water resistance, etc., achieve good anti-aging effect, simple preparation method, Fast curing effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] The preparation method of vest bag dispensing glue comprises the steps:
[0027] 1) be 20 parts by weight of rosin resin, 10 parts of liquid paraffin, 1 part of silane coupling agent and 1 part of di-tert-butyl p-cresol and [β-(3,5-di-tert-butyl Base 4-hydroxyphenyl) propionic acid] pentaerythritol ester compound system mixed and stirred, heated to a molten state; the heating temperature is 160 ~ 170 ° C, the stirring speed is controlled at 100 rpm;
[0028] 2) be 15 parts of ethylene-vinyl acetate copolymers and 15 parts of styrene-butadiene block copolymers in parts by weight, 3 parts of silane coupling agent KH-560 modified nano silicon dioxide, 5 parts Parts of dibutyl phthalate, 1 part of di-tert-butyl p-cresol and [β-(3,5-di-tert-butyl 4-hydroxyphenyl) propionic acid] pentaerythritol compound system mixed, Add the mixture in step 1) and heat and stir until it melts; the heating temperature is 160-170°C, and the stirring speed is controlled at 100 rpm;
[0029] 3...
Embodiment 2
[0031] The preparation method of vest bag dispensing glue comprises the steps:
[0032] 1) be 20 parts by weight of rosin resin, 30 parts of terpene resin, 15 parts of liquid paraffin, 3 parts of di-tert-butyl p-cresol and [β-(3,5-di-tert-butyl Mix and stir the compound system of 4-hydroxyphenyl)propionic acid]pentaerythritol ester, and heat to a molten state; the heating temperature is 160-170°C, and the stirring speed is controlled at 200 rpm;
[0033] 2) 20 parts by weight of ethylene-vinyl acetate copolymer and 5 parts of styrene-butadiene block copolymer, 3 parts of silane coupling agent KH-560 modified nano silicon dioxide, 5 parts Parts of dibutyl phthalate, 2 parts of di-tert-butyl p-cresol and [β-(3,5-di-tert-butyl 4-hydroxyphenyl) propionic acid] pentaerythritol compound system mix, Add the mixture in step 1) and heat and stir until it melts; the heating temperature is 160-170°C, and the stirring speed is controlled at 150 rpm;
[0034] 3) When the mixture forms a ...
Embodiment 3
[0036] The preparation method of vest bag dispensing glue comprises the steps:
[0037] 1) be 25 parts by weight of C5 petroleum resin, 10 parts of terpene resin, 15 parts of lanolin, 1.5 parts of di-tert-butyl-p-cresol and [β-(3,5-di-tert-butyl Base 4-hydroxyphenyl) propionic acid] pentaerythritol ester compound system mixed and stirred, heated to a molten state; the heating temperature is 160 ~ 170 ° C, the stirring speed is controlled at 60 rpm;
[0038] 2) be 5 parts of ethylene-vinyl acetate copolymers and 25 parts of styrene-butadiene block copolymers by weight, 1 part of silane coupling agent KH-560 modified nano silicon dioxide, 5 parts 1 part of naphthenic oil, 2 parts of di-tert-butyl-p-cresol and [β-(3,5-di-tert-butyl 4-hydroxyphenyl) propionic acid] pentaerythritol ester mixed, add step 1) Heat and stir the mixture until it melts; the heating temperature is 160-170°C, and the stirring speed is controlled at 80 rpm;
[0039] 3) When the mixture forms a uniform and...