Embodiment 1
[0061] An attapulgite-based organic soil conditioner, comprising the following preparation steps:
[0062] A. Raw ore crushing
[0063] Crush the attapulgite ore and eggshell, the broken mesh is 30 mesh-60 mesh;
[0064] B. Acidification treatment
[0065] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0066] C. Drying and sieving
[0067] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0068] D. Baking
[0069] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time is 45-12...
Embodiment 2
[0077] An attapulgite-based organic soil conditioner, comprising the following preparation steps:
[0078] A. Raw ore crushing
[0079] Crush the attapulgite ore and eggshell, the crushing mesh number is 30 mesh-60 mesh;
[0080] B. Acidification treatment
[0081] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0082] C. Drying and sieving
[0083] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0084] D. Baking
[0085] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time...
Embodiment 3
[0095] An attapulgite-based organic soil conditioner, comprising the following preparation steps:
[0096] A. Raw ore crushing
[0097] Crush the attapulgite ore and eggshell, the broken mesh is 30 mesh-60 mesh;
[0098] B. Acidification treatment
[0099] Concentrated sulfuric acid with a mass fraction of 98% was added to the water to prepare a sulfuric acid solution with a molar concentration of 1 to 3 mol / L, and the sulfuric acid solution was added to the attapulgite ore broken in step A, and acidified for 4 hours to make attapulgite clay;
[0100] C. Drying and sieving
[0101] Airing the acidified attapulgite clay, drying to reduce the water content of the attapulgite clay to 15%, then crushing and sieving to obtain attapulgite powder, the mesh size of the attapulgite is 100-150 mesh;
[0102] D. Baking
[0103] Send the screened attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300-360°C, and the roasting time is 45-12...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com