Processing process of washable cowhide garment leather
A processing technology and garment leather technology, which is applied in the field of garment fabric processing, can solve the problems of high price, hard feeling, complicated tanning process, etc., and achieve the effect of environmental protection, high mechanical strength and simple process in the tanning process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] A kind of water-resistant cowhide garment leather processing technology provided by the present embodiment, said water-washable cowhide garment leather processing technology comprises the following steps:
[0033] (1) Cowhide pre-treatment: Check the cowhide to see if there are cracks in the leather board, whether the folds are rotten and hair loss, sew up the cracks, cut off the rotten parts, remove the sundries stuck to the cowhide, and then soak and cook after suturing ;
[0034] (2) Soaking: Soak cowhide with water for 1 day in summer and 2-3 days in winter;
[0035] (3) deashing;
[0036] (4) pickling: put the cowhide after deliming into the hydrochloric acid solution with a mass fraction of 10% and soak for 2-4h, and the volume ratio of the cowhide to the hydrochloric acid solution is 1:4;
[0037] (5) Tanning: Add 4.2% aluminum tanning agent to the acid solution of step (4), soak for 30 minutes, then add 0.8% sodium formate, soak for 30 minutes, then add 0.6% b...
Embodiment 2
[0052] A kind of water-resistant cowhide garment leather processing technology provided by the present embodiment, said water-washable cowhide garment leather processing technology comprises the following steps:
[0053] (1) Cowhide pre-treatment: Check the cowhide to see if there are cracks in the leather board, whether the folds are rotten and hair loss, sew up the cracks, cut off the rotten parts, remove the sundries stuck to the cowhide, and then soak and cook after suturing ;
[0054] (2) Soaking: Soak cowhide with water for 1 day in summer and 2-3 days in winter;
[0055] (3) deashing;
[0056] (4) pickling: put the cowhide after deliming into the hydrochloric acid solution with a mass fraction of 10% and soak for 2-4h, and the volume ratio of the cowhide to the hydrochloric acid solution is 1:2;
[0057] (5) Tanning: Add 3.0% aluminum tanning agent to the acid solution of step (4), soak for 30 minutes, then add 1.3% sodium formate, soak for 30 minutes, then add 0.3% b...
Embodiment 3
[0072] A kind of water-resistant cowhide garment leather processing technology provided by the present embodiment, said water-washable cowhide garment leather processing technology comprises the following steps:
[0073] (1) Cowhide pre-treatment: Check the cowhide to see if there are cracks in the leather board, whether the folds are rotten and hair loss, sew up the cracks, cut off the rotten parts, remove the sundries stuck to the cowhide, and then soak and cook after suturing ;
[0074] (2) Soaking: Soak cowhide with water for 1 day in summer and 2-3 days in winter;
[0075] (3) deashing;
[0076] (4) pickling: put the cowhide after deliming into the hydrochloric acid solution with a mass fraction of 10% and soak for 2-4h, and the volume ratio of the cowhide to the hydrochloric acid solution is 1:2-4;
[0077] (5) Tanning: Add 3.5% aluminum tanning agent to the acid solution of step (4), soak for 30 minutes, then add 0.9% sodium formate, soak for 30 minutes, then add 0.5%...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com