Sponge for body armor and preparation method thereof
A bulletproof vest and sponge technology, applied in the field of sponges, can solve the problems of large concave deformation of tensile strength, decreased flexibility of the wearer, uncomfortable wearer, etc., and achieves high tensile strength and tear strength, fine pore size, slow rebound effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0049] A kind of sponge for body armor, comprising by weight parts:
[0050] 25 parts of polyether polyols;
[0051] 25 parts of polymer polyols;
[0052] Slow rebound polyether 40 parts;
[0053] 17 TDIs;
[0054] 1.5 parts of amine catalyst;
[0055] 0.04 part of tin catalyst;
[0056] Tension agent 1.4 parts;
[0057] 0.7 parts of toughening agent;
[0058] 0.6 parts of silicone oil;
[0059] 0.5 parts of water.
[0060] The polyether polyol has a hydroxyl value of 60 mgKOH / g and a molecular weight of 2500; the polymer polyol has a solid content of 43%; the slow resilience polyether has a hydroxyl value of 230 mgKOH / g and a molecular weight of 2300.
[0061] The preparation method of the sponge for body armor is as follows: polyether polyol, polymer polyol, slow rebound polyether, amine catalyst, tin catalyst, tensile agent, toughening agent, silicone oil, water are mixed in proportion, in 50000 Stir for 10-20s at the speed of rpm, atomize and inject TDI at a high ...
Embodiment 2
[0063] A kind of sponge for body armor, comprising by weight parts:
[0064] 40 parts of polyether polyols;
[0065] 15 parts of polymer polyols;
[0066] Slow rebound polyether 50 parts;
[0067] 23 TDIs;
[0068] 3 parts of amine catalyst;
[0069] Tin catalyst 0.07
[0070] Tension agent 1.8 parts;
[0071] 1.6 parts of toughening agent;
[0072] 0.8 parts of silicone oil;
[0073] 0.6 parts of water.
[0074] The polyether polyol has a hydroxyl value of 55 mgKOH / g and a molecular weight of 2800; the polymer polyol has a solid content of 48%; the slow resilience polyether has a hydroxyl value of 230 mgKOH / g and a molecular weight of 1900.
[0075] The preparation method of Example 2 is the same as that of Example 1, and the specific steps are shown in Example 1, which will not be repeated here.
Embodiment 3
[0077] A kind of sponge for body armor, comprising by weight parts:
[0078] 25 parts of polyether polyols;
[0079] 15 parts of polymer polyols;
[0080] Slow rebound polyether 40 parts;
[0081] TDI 15 copies;
[0082] 1.2 parts of amine catalyst;
[0083] Tin catalyst 0.03 parts
[0084] Tension agent 1 part;
[0085] 1 part of toughening agent;
[0086] 0 parts of silicone oil;
[0087] 0.4 parts of water.
[0088] The polyether polyol has a hydroxyl value of 50 mgKOH / g and a molecular weight of 3200; the polymer polyol has a solid content of 40%; the slow resilience polyether has a hydroxyl value of 240 mgKOH / g and a molecular weight of 2400.
[0089] The preparation method of Example 3 is the same as that of Example 1, and the specific steps are shown in Example 1, and will not be repeated here.
PUM
Property | Measurement | Unit |
---|---|---|
hydroxyl value | aaaaa | aaaaa |
hydroxyl value | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com