Fireproof coating, antique wooden hanging plate and preparation method of antique wooden hanging plate
A fire-resistant coating and wood-based technology, which is applied in the direction of fire-resistant coatings, coatings, and devices for coating liquids on the surface, can solve problems such as poor fire-proof performance, and achieve good machine-automated coating effects, high fire-proof performance, and fluidity Good results
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] Raw materials: 20 parts of amino resin; 5 parts of ethylene glycol butyl ether; 0.2 parts of alcohol ester-12; 0.2 parts of benzyl alcohol; 0.15 parts of water-based polyurethane dispersion; ; 5 parts of phosphonate, 6 parts of phosphate nitrogen phosphate, 6 parts of guanidine phosphate and 2 parts of zirconium borate; 11 parts of pentaerythritol; 5 parts of phytic acid; 1 part of triethanolamine; 5 parts of wood stabilizer MJB-TF; color paste 5 parts; 35 parts of water.
[0033] Preparation of fire retardant coatings
[0034] Include the following steps:
[0035] Step 1. Mix the above-mentioned raw materials in proportion, carry out the first stirring for 20 minutes, and the rotation speed is 1000r / min, and then leave it for 2 hours to obtain the first material;
[0036] Step 2. Stir the first material obtained in step 1 for a second time under the action of ultrasound with a frequency of 100KHz at a speed of 1500r / min, and stop after 10min to obtain a fireproof coa...
Embodiment 2
[0044] Raw materials: 22 parts of amino resin; 6 parts of ethylene glycol butyl ether; 0.1 part of alcohol ester-12; 0.1 part of benzyl alcohol; 0.2 parts of water-based polyurethane dispersion; 4 parts of ethylene-ethylene acetate copolymer; 5 parts of polysiloxane ; 5 parts of phosphonate, 7 parts of phosphorus nitrogen phosphate, 8 parts of guanidine phosphate and 1 part of zirconium borate; 10 parts of pentaerythritol; 5 parts of phytic acid; 1.0 part of triethanolamine; 6 parts of wood stabilizer MJB-TF; ; 45 parts of water.
[0045] Preparation of fire retardant coatings
[0046] Include the following steps:
[0047] Step 1. Mix the above-mentioned raw materials in proportion, carry out the first stirring for 15 minutes, and the rotation speed is 800r / min, and then stand still for 1 hour to obtain the first material;
[0048] Step 2. Stir the first material obtained in step 1 for a second time under the action of ultrasound with a frequency of 80KHz at a speed of 1200r...
Embodiment 3
[0056] Raw materials: 18 parts of amino resin; 4 parts of ethylene glycol butyl ether; 0.05 part of alcohol ester-12; 0.05 part of benzyl alcohol; 0.1 part of water-based polyurethane dispersion; 3 parts of ethylene-ethylene acetic acid copolymer; ; 5 parts of phosphonate, 6 parts of phosphate nitrogen phosphate, 7 parts of guanidine phosphate and 2 parts of zirconium borate; 9 parts of pentaerythritol; 3 parts of phytic acid; 1 part of triethanolamine; 5 parts of wood stabilizer MJB-TF; 3 parts of color paste parts; 30 parts of water.
[0057] Preparation of fire retardant coatings
[0058] Include the following steps:
[0059] Step 1. Mix the above-mentioned raw materials in proportion, carry out the first stirring for 12 minutes, and the rotation speed is 700r / min, and then stand still for 1 hour to obtain the first material;
[0060] Step 2. Stir the first material obtained in step 1 for a second time under the action of ultrasound with a frequency of 60KHz at a speed of...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More