House earth surface sectional material and manufacturing method thereof
A profile and floor technology, applied in chemical instruments and methods, floors, building structures, etc., can solve the problems of easy-to-expand deformed floors, high thermal expansion coefficient, unsightly, etc., to ensure structural strength and durability, and improve economical efficiency. The effect of high value and product qualification rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] The floor profile of the house according to the present invention has the main components of the inner layer material in parts by weight:
[0034] 100 parts of PVC, 0.8 parts of azodicarbonamide, 6 parts of composite stabilizer, the composite stabilizer is barium stearate, stearic acid, ultraviolet absorber (UV-531), dibasic lead stearate, dibasic A mixture of lead phosphite, calcium stearate and paraffin, the weight ratio is: 8:10:1:12:70:20:1; 9 parts of acrylate; CaCO 3 5 copies;
[0035] The main components of the outer layer material are in parts by weight:
[0036] Accessory 1: 100 parts of PVC, 30 parts of bran powder and ASA resin (30:70 by weight) passed through a 120-mesh sieve, 5.5 parts of composite stabilizer, which is barium stearate, stearic acid, and ultraviolet absorber (UV-531), a mixture of dibasic lead stearate, dibasic lead phosphite, calcium stearate and paraffin, the weight ratio of which is: 8:10:1:12:70:20:1; 0.8 parts of LIGA, 0.8 parts of a...
Embodiment 2
[0043] The floor profile of the house according to the present invention has the main components of the inner layer material in parts by weight:
[0044] 100 parts of PVC, 1 part of azodicarbonamide, 5.5 parts of composite stabilizer, composite stabilizer is stearic acid, ultraviolet absorber (UV-326), dibasic lead stearate, dibasic lead phosphite, The mixture of calcium stearate and paraffin, its weight ratio is: 10:1:12:70:20:1, 9 parts of acrylates;
[0045] The main components of the outer layer material are in parts by weight:
[0046] Accessory 1: 100 parts of PVC, 30 parts of wood flour and ASA resin (40:60 by weight) passed through a 100-mesh sieve, 6 parts of composite stabilizer, which is stearic acid and ultraviolet absorber (UV-326) , a mixture of dibasic lead stearate, dibasic lead phosphite, calcium stearate and paraffin, the weight ratio of which is: 10:1:12:70:20:1; 381 parts of LIGA, azodicarbonamide 0.8 parts, 3 parts of rutile titanium dioxide;
[0047] E...
Embodiment 3
[0053] The floor profile of the house of the present invention, the proportioning of its inner and outer layer materials is:
[0054] The main components of the inner material of the profile are in parts by weight:
[0055]100 parts of PVC, 0.9 parts of azodicarbonamide, 6 parts of composite stabilizer, composite stabilizer is stearic acid, ultraviolet absorber (UV-3346), dibasic lead stearate, dibasic lead phosphite and The mixture of calcium stearate, its weight ratio is: 10:1:12:70:20; 8 parts of acrylate; CaCO 3 7 copies
[0056] The main components of the outer layer material are in parts by weight:
[0057] Accessory 1: 100 parts of PVC, 30 parts of rice husk powder and ASA resin (weight ratio of 20:80) through 80 mesh sieve, 6 parts of composite stabilizer, composite stabilizer is stearic acid, ultraviolet absorber (UV-3346 ), a mixture of dibasic lead stearate, dibasic lead phosphite and calcium stearate, the weight ratio of which is: 10:1:12:70:20; 1 part of KZTPP,...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com