Curing agent for sludge solidification and stabilization and preparation and application thereof
A technology of sludge solidification and solidifying agent, applied in chemical instruments and methods, fixed/solidified sludge treatment, water/sludge/sewage treatment, etc., can solve problems such as unsuitable site search, limited landfill capacity, and unsafety. , to achieve the effect of simplifying the treatment process and difficulty, shortening the maintenance period, and reducing the treatment cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0043] In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0044] Portland cement 20%,
[0045] Fly ash 30%,
[0046] Quicklime 30%,
[0048] Aluminum and calcium salts 5%,
[0049] Wherein, the aluminum salt is aluminum sulfate, the calcium salt is calcium chloride, and the mass ratio of aluminum sulfate to calcium chloride is 3:1.
[0050] Application of the above-mentioned curing agent: Add 500 kg of the above-mentioned curing agent to the original sludge with a moisture content as high as 96.3% per ton, and the strength can reach 143 kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. . After testing, the leachate concentration of heavy metals meets the identification standard of leaching toxicity.
Embodiment 2
[0052] In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0053] Portland cement 40%,
[0054] Fly Ash 10%,
[0055] Quicklime 30%,
[0057] Aluminum and calcium salts 5%,
[0058] Wherein, the aluminum salt is aluminum sulfate, the calcium salt is calcium chloride, and the mass ratio of aluminum sulfate to calcium chloride is 3:1.
[0059] Application of the above-mentioned curing agent: add 450kg of the above-mentioned curing agent to the raw sludge with a moisture content as high as 96.3% per ton, and the strength can reach 151kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. After testing, the leachate concentration of heavy metals meets the identification standard of leaching toxicity.
Embodiment 3
[0061]In this example, the solidification agent used for solidification and stabilization of the sludge in the sludge plant is mixed according to the following formula (percentage by weight):
[0062] Portland cement 40%,
[0063] Fly Ash 10%,
[0064] Quicklime: 10%,
[0065] Ferrous sulfate: 30%,
[0066] Aluminum and calcium salts: 10%,
[0067] Wherein, the aluminum salt is aluminum chloride, the calcium salt is calcium sulfate, and the mass ratio of aluminum chloride to calcium sulfate is 1:1.
[0068] Application of the above-mentioned curing agent: add 450 kg of the above-mentioned curing agent to the original sludge with a moisture content as high as 96.3% per ton, and the strength can reach 137kPa after 4 days, which meets the strength requirements of landfill disposal and construction fill. The concentration detection of the leach solution of heavy metals complied with the identification standard of leaching toxicity.
PUM
| Property | Measurement | Unit |
|---|---|---|
| Strength | aaaaa | aaaaa |
| Strength | aaaaa | aaaaa |
| Strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com