The technology of a dust suppressant and defoamer, which is applied in the field of defoaming dust suppressant and its preparation, can solve problems such as mine safety production accidents, excessive foam, and affecting the effect of spray dust suppression, so as to ensure normal and safe operation and improve dust suppression. Efficiency, the effect of ensuring homogeneity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0050] As an embodiment of the present invention, the preparation method of the dust suppressant includes the following steps:
[0051] 1) Weigh 2.2g of OP-20 and dissolve it in 10g of deionized water and dissolve it completely for use; in addition, weigh out 2.05g of sodium dodecylbenzene sulfonate and dissolve it in 10g of deionized water and dissolve it for use; then Mix the two, after standing for 20 minutes, then add 9.08g of deionized water to the mixed solution, and stand for 10 minutes to obtain the first solution (A1) for use;
[0052] 2) Weigh 2.84 g of ethylene glycol and dissolve it in 20 g of deionized water. After it is completely dissolved, add 10.49 g of deionized water and let it stand for 15 minutes to obtain the second solution (B1) for use;
[0053] 3) Weigh 2.75g of sodium silicate and dissolve it in 20g of deionized water, add 10.58g of deionized water after it is completely dissolved, and let it stand for 10 minutes to obtain the third solution (C1) for use;
[...
Embodiment 2
[0056] As an embodiment of the present invention, the preparation method of the dust suppressant includes the following steps:
[0057] 1) Weigh 0.95g of AEO-9 and dissolve it in 10g of deionized water, and dissolve it completely for use; in addition, weigh 1.50g of sodium dodecyl sulfonate and dissolve it in 10g of deionized water, and dissolve it for use; After mixing, add 10.88g of deionized water and let stand for 8 minutes to obtain the first solution (A2), which is ready for use;
[0058] 2) Weigh 0.85g of ethanol and dissolve it in 20g of deionized water. After it is completely dissolved, add 12.48g of deionized water and let it stand for 15 minutes to obtain the second solution (B2) for use;
[0059] 3) Weigh 0.65g of potassium sulfate and dissolve it in 20g of deionized water, add 12.68g of deionized water after it is completely dissolved, and let it stand for 18 minutes to obtain the third solution (C3) for use;
[0060] 4) The first solution (A2), the second solution (B2), ...
Embodiment 3
[0062] 1) Weigh 0.55g TX-7 and dissolve it in 10g deionized water and dissolve it completely for use; in addition, weigh 1.50g sodium dodecylbenzene sulfonate and dissolve it in 10g deionized water, and dissolve it for use; then Mix the two, then add 11.25g of deionized water, and let it stand for 8 minutes to obtain the first solution (A3), ready for use;
[0063] 2) Weigh 1.95g polyethylene glycol, dissolve it in 20g deionized water, add 11.38g deionized water and let it stand for 15min to obtain the second solution (B3) for use;
[0064] 3) Weigh 2.05g of strontium carbonate and dissolve it in 20g of deionized water, add 11.28g of deionized water after complete dissolution, and let it stand for 22 minutes to obtain the third solution (C3) for use;
[0065] 4) Mix the first solution (A3), the second solution (B3), and the third solution (C3) uniformly, and then prepare the dust suppressant (dust suppressant 3) after standing for 10 minutes.