Ultrasonic iron removal technology of quartz sand
A quartz sand and ultrasonic technology, applied in the field of quartz sand purification, can solve the problems of low iron removal efficiency, long cleaning time, and inability to remove impurities in quartz sand particles, and achieve high iron removal efficiency and short cleaning time.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] The ultrasonic iron removal process of the quartz sand of embodiment 1 may further comprise the steps:
[0017] S1: Put quartz sand in a reactor, add oxalic acid solution into the reactor, ultrasonically oscillate and stir, heat to 80°C, react for 10 minutes, and filter to obtain solid quartz sand;
[0018] S2: wash the quartz sand solid obtained in S1 with distilled water, and put it into an oven for drying;
[0019] The concentration of oxalic acid in the oxalic acid solution in S1 is 4g / L.
[0020] Wherein, the frequency of the ultrasonic wave is 40 KHz.
[0021] Wherein, the stirring speed is 300r / min.
[0022] Among them, the fineness of quartz sand is 80-90 mesh.
Embodiment 2
[0024] The ultrasonic iron removal process of the quartz sand of embodiment 2 may further comprise the steps:
[0025] S1: Put quartz sand in a reactor, add oxalic acid solution into the reactor, ultrasonically oscillate and stir, heat to 120°C, react for 20 minutes, and filter to obtain solid quartz sand;
[0026] S2: wash the quartz sand solid obtained in S1 with distilled water, and put it into an oven for drying;
[0027] The concentration of oxalic acid in the oxalic acid solution in S1 is 6g / L.
[0028] Wherein, the frequency of the ultrasonic wave is 50 KHz.
[0029] Wherein, the stirring speed is 500r / min.
[0030] Among them, the fineness of quartz sand is 90-100 mesh.
Embodiment 3
[0032] The ultrasonic iron removal process of the quartz sand of embodiment 3 may further comprise the steps:
[0033] S1: Put quartz sand in a reactor, add oxalic acid solution into the reactor, ultrasonically oscillate and stir, heat to 100°C, react for 15 minutes, and filter to obtain solid quartz sand;
[0034] S2: wash the quartz sand solid obtained in S1 with distilled water, and put it into an oven for drying;
[0035] The concentration of oxalic acid in the oxalic acid solution in S1 is 5g / L.
[0036] Wherein, the frequency of the ultrasonic wave is 45KHz.
[0037] Wherein, the stirring speed is 400r / min.
[0038] Among them, the fineness of quartz sand is 85-95 mesh.
[0039] Generally, iron impurity particles are distributed in three ways in quartz sand: one is adsorbed on the surface of quartz sand particles; the other is embedded in quartz sand particles; the third is contained in the interior of quartz sand particles. After ultrasonic cleaning, these cracked q...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com