Oil agent for natural fibers and preparation method of oil agent
A technology of natural fiber and oil agent, applied in the direction of natural fiber, fiber treatment, fiber type, etc., can solve the problem of poor carding passability and antistatic performance, spinning bundle, poor drafting, and large influence of temperature and humidity, etc. problem, to achieve the effect of significant softening effect, good antistatic effect and increasing penetration effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] An oil agent for natural fiber textiles, comprising the following raw materials in parts by weight: 8 parts of alkylphenol polyoxyethylene ether, 6 parts of fatty alcohol sodium sulfate, 5 parts of lauryl betaine, 3 parts of polyethylene glycol laurate 2 parts, 2 parts of ammonium persulfate, 2 parts of silicone, 5 parts of vegetable oil, 1 part of sorbic acid, 2 parts of glycerin, 1 part of polyethylene glycol oleate, 60 parts of deionized water.
[0017] A preparation method for natural fiber oil, comprising the following steps:
[0018] a. Take 30 parts of deionized water and heat it to 35°C, keep the temperature constant, then add alkylphenol polyoxyethylene ether, fatty alcohol sodium sulfate, vegetable oil, sorbic acid and glycerin in sequence, and stir for 30 minutes;
[0019] b. Take 30 parts of deionized water and heat it to 50°C, then add lauryl betaine, polyethylene glycol laurate, ammonium persulfate, silicone and polyethylene glycol oleate in sequence, and ...
Embodiment 2
[0022] An oil agent for natural fiber textiles, comprising the following raw materials in parts by weight: 10 parts of alkylphenol polyoxyethylene ether, 10 parts of sodium dodecylbenzenesulfonate, 6 parts of lauryl betaine, polyethylene glycol 5 parts of laurate, 4 parts of ammonium persulfate, 3 parts of silicone, 8 parts of vegetable oil, 3 parts of sorbic acid, 4 parts of glycerin, 2 parts of polyethylene glycol oleate, 80 parts of deionized water.
[0023] A preparation method for natural fiber oil, comprising the following steps:
[0024] a. Take 40 parts of deionized water and heat it to 40°C, keep the temperature constant, then add alkylphenol polyoxyethylene ether, fatty alcohol sodium sulfate, vegetable oil, sorbic acid and glycerin in sequence, and stir for 40 minutes;
[0025] b. Take 40 parts of deionized water and heat it to 60°C, then add lauryl betaine, polyethylene glycol laurate, ammonium persulfate, silicone and polyethylene glycol oleate in sequence, and ke...
Embodiment 3
[0028] An oil agent for natural fiber textiles, comprising the following raw materials in parts by weight: 14 parts of alkylphenol polyoxyethylene ethers, 12 parts of hydroxyalkylphenol polyoxyethylene ethers, 8 parts of lauryl betaine, polyethylene glycol 8 parts of laurate, 6 parts of ammonium persulfate, 5 parts of silicone, 10 parts of vegetable oil, 5 parts of sorbic acid, 7 parts of glycerin, 3 parts of polyethylene glycol oleate, 100 parts of deionized water.
[0029] A preparation method for natural fiber oil, comprising the following steps:
[0030] a. Take 50 parts of deionized water and heat it to 50°C, keep the temperature constant, then add alkylphenol polyoxyethylene ether, fatty alcohol sodium sulfate, vegetable oil, sorbic acid and glycerin in sequence, and stir for 45 minutes;
[0031] b. Take 50 parts of deionized water and heat it to 80°C, then add lauryl betaine, polyethylene glycol laurate, ammonium persulfate, silicone and polyethylene glycol oleate in se...