An anti-ultraviolet and ultraviolet technology, applied in glass manufacturing equipment, glass forming, glass calendering and other directions, can solve the problems of low resistance performance, low aging, and the UV resistance of patterned glass needs to be improved, and achieve good flame retardant and anti- The effect of fog performance, strong ability to resist UV rays
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0012] An anti-ultraviolet patterned glass, made of the following raw materials in parts by mass: 20 parts of silicon dioxide, 20 parts of calcium silicate, 10 parts of sodium silicate, 10 parts of methyl methacrylate, 6 parts of brominated epoxy resin 3 parts of diethanolamine, 6 parts of titanium dioxide, 3 parts of ultraviolet absorber, 1 part of glycerol diacetate, 2 parts of iron oxide, 0.1 part of dichromate, 0.5 part of ferrous oxide, and 0.05 part of auxiliary agent.
[0013] The ultraviolet absorber is 2-hydroxyl-4-methoxybenzophenone. The titanium dioxide is prepared by mixing anatase titanium dioxide and rutile titanium dioxide at a mass ratio of 1:1. The auxiliary agent is isopropanol.
[0014] A method for preparing UV-resistant embossed glass, comprising the following steps: (1) according to 20 parts of silicon dioxide, 20 parts of calcium silicate, 10 parts of sodium silicate, 10 parts of methyl methacrylate, brominated epoxy 6 parts of resin, 3 parts of dieth...
Embodiment 2
[0016] An anti-ultraviolet patterned glass, made of the following raw materials in parts by mass: 25 parts of silicon dioxide, 23 parts of calcium silicate, 15 parts of sodium silicate, 13 parts of methyl methacrylate, and 7 parts of brominated epoxy resin 5 parts of diethanolamine, 8 parts of titanium dioxide, 8 parts of ultraviolet absorber, 2 parts of glycerin diacetate, 3 parts of iron oxide, 0.3 part of dichromate, 1 part of ferrous oxide, and 0.08 part of auxiliary agent.
[0017] The ultraviolet absorber is 2-hydroxyl-4-n-octyloxybenzophenone. The titanium dioxide is prepared by mixing anatase titanium dioxide and rutile titanium dioxide at a mass ratio of 1:1. The auxiliary agent is xylitol ester.
[0018] A method for preparing UV-resistant embossed glass, comprising the following steps: (1) according to 25 parts of silicon dioxide, 23 parts of calcium silicate, 15 parts of sodium silicate, 13 parts of methyl methacrylate, brominated epoxy 7 parts of resin, 5 parts ...
Embodiment 3
[0020] An anti-ultraviolet patterned glass, made of the following raw materials in parts by mass: 30 parts of silicon dioxide, 26 parts of calcium silicate, 15 parts of sodium silicate, 13 parts of methyl methacrylate, 8 parts of brominated epoxy resin 5 parts of diethanolamine, 8 parts of titanium dioxide, 12 parts of ultraviolet absorber, 3 parts of glycerol diacetate, 3 parts of iron oxide, 0.3 part of dichromate, 1.5 parts of ferrous oxide, and 1 part of additive.
[0021] The ultraviolet absorber is 2-hydroxyl-4-n-octyloxybenzophenone. The titanium dioxide is prepared by mixing anatase titanium dioxide and rutile titanium dioxide at a mass ratio of 1.5:1. The auxiliary agent is isopropanol.
[0022] A method for preparing UV-resistant embossed glass, comprising the following steps: (1) according to 30 parts of silicon dioxide, 26 parts of calcium silicate, 15 parts of sodium silicate, 13 parts of methyl methacrylate, brominated epoxy 8 parts of resin, 5 parts of diethan...