A cubic silicon carbide oil, cubic silicon carbide technology, used in the manufacture of tools, ceramic products, metal processing equipment, etc., can solve the problem of improper matching of process parameters such as sintering temperature and molding pressure, and it is difficult to achieve hardness uniformity and durability. Meet production needs and other issues to achieve better finish, improved grinding finish, and controllable porosity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] The preparation process of the cubic silicon carbide oilstone formula of the present invention comprises the following steps:
[0027] A. Ingredients:
[0028] Cubic silicon carbide is used as abrasive material, potassium feldspar is used as melting material, refined naphthalene is used as pore-forming agent, dextrin is used as bonding lubricant, boron glass is used as sintering aid, and kaolin which can improve plasticity is added. 95 parts, potassium feldspar 20 parts, refined naphthalene 9 parts, talcum powder 6 parts, dextrin 3 parts, sugar water 23 parts, boron glass 5 parts, the raw material composition of 13 parts of kaolin and weight carry out weighing proportioning; Said Refined naphthalene is ground before adding ingredients, and then sieved to make fine particles;
[0029] B. Mixing:
[0030] The weighed various raw materials are mixed uniformly in a planetary ball mill, the ball milling medium is agate balls, the ratio of material to ball is 3: 1, the mixt...
Embodiment 2
[0042] The preparation process of the cubic silicon carbide oilstone formula of the present invention comprises the following steps:
[0043] A. Ingredients:
[0044] Cubic silicon carbide is used as abrasive material, potassium feldspar is used as melting material, refined naphthalene is used as pore-forming agent, dextrin is used as bonding lubricant, boron glass is used as sintering aid, and kaolin which can improve plasticity is added. 98 parts, 28 parts of potassium feldspar, 10 parts of refined naphthalene, 6 parts of talcum powder, 4 parts of dextrin, 25 parts of syrup, 6 parts of boron glass, 14 parts of kaolin are weighed and proportioned; Refined naphthalene is ground before adding ingredients, and then sieved to make fine particles;
[0045] B. Mixing:
[0046] The weighed various raw materials are mixed uniformly in a planetary ball mill, the ball milling medium is agate balls, the ratio of material to ball is 3: 1, the mixture is mixed for 3.5 hours and sieved t...
Embodiment 3
[0058] The preparation process of the cubic silicon carbide oilstone formula of the present invention comprises the following steps:
[0059] A. Ingredients:
[0060] Cubic silicon carbide is used as abrasive material, potassium feldspar is used as catalyzed raw material, refined naphthalene is used as pore-forming agent, dextrin is used as bonding lubricant, boron glass is used as sintering aid, and kaolin which can improve plasticity is added. 100 parts, 35 parts of potassium feldspar, 11 parts of refined naphthalene, 7 parts of talcum powder, 5 parts of dextrin, 28 parts of syrup, 8 parts of boron glass, 15 parts of kaolin raw material composition and weight carry out weighing proportioning; Said Refined naphthalene is ground before adding ingredients, and then sieved to make fine particles;
[0061] B. Mixing:
[0062] The various raw materials weighed are mixed uniformly in a planetary ball mill, and the ball milling medium is agate balls, the ratio of material to ball ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com