A method for preparing solid waste base geopolymers by using the stuffy slag method in conjunction with red mud

A technology of polymer glue and polymer material, applied in cement production and other directions, can solve problems such as high temperature calcination, and achieve the effect of alleviating environmental problems, convenient application, and eliminating calcination process.

Active Publication Date: 2019-01-25
SHANDONG UNIV
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

After mixing Bayer process red mud, coal gangue, and alkali metal materials, they are mixed with molten steel slag, and activated through the slag process in the steel slag treatment process to improve the activity of silicon and aluminum, and prepare a product that can be directly formed by adding water and stirring naturally. Geopolymer cementitious materials, thus solving the problem that the geopolymer cementitious materials produced by the Bayer process red mud need high-temperature calcination, red mud needs to be filtered and evaporated to remove water, and the curing process requires autoclave or dry molding technologies. question

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0033] The method for preparing the solid waste base geopolymer by using the stuffy slag method in cooperation with the red mud comprises the following steps:

[0034] (1) drying the coal gangue until the moisture content is less than 1%, grinding, and passing through a 100-mesh sieve;

[0035] (2) Take 100 parts of steel slag in each converter, weigh 30 parts of coal gangue powder, 20 parts of sodium hydroxide, 10 parts of water glass and 160 parts of water-containing red mud and evenly mix;

[0036] (3) The mixture is fully mixed with 40 parts of molten steel slag, and the mixture is calcined for 1.5 hours by the slag method at a temperature of 750° C.;

[0037] (4) Grinding the calcined mixture until the specific surface area is 360-400m 2 / kg to obtain solid waste base geopolymer materials.

[0038] When preparing the geopolymer gelling material, directly add 30% of the total mass of water and stir evenly, pour it into a 40×40×160 mold, place it in a curing box at 20°C a...

Embodiment 2

[0040] The method for preparing the solid waste base geopolymer by using the stuffy slag method in cooperation with the red mud comprises the following steps:

[0041] (1) drying the coal gangue until the moisture content is less than 1%, grinding, and passing through a 100-mesh sieve;

[0042] (2) Take 100 parts of steel slag in every converter, weigh 40 parts of coal gangue powder, 25 parts of sodium hydroxide, 10 parts of water glass and 120 parts of water-containing red mud, and mix evenly.

[0043] (3) The mixture is fully mixed with 60 parts of molten steel slag, and the mixture is calcined for 2 hours by the slag method at a temperature of 850° C.;

[0044] (4) Grinding the calcined mixture until the specific surface area is 360-400m 2 / kg to obtain solid waste base geopolymer materials.

[0045] The geopolymer gelling material is directly mixed with 70% of the total mass of water and stirred evenly, poured into a mold of 40×40×160, placed in a curing box at 20°C and ...

Embodiment 3

[0047] The method for preparing the solid waste base geopolymer by using the stuffy slag method in cooperation with the red mud comprises the following steps:

[0048] (1) drying the coal gangue until the moisture content is less than 1%, grinding, and passing through a 100-mesh sieve;

[0049] (2) Take 100 parts of steel slag in every converter, weigh 50 parts of coal gangue powder, 25 parts of sodium hydroxide, 10 parts of water glass and 120 parts of water-containing red mud and mix evenly,

[0050] (3) The mixture is fully mixed with 60 parts of molten steel slag, and the mixture is calcined for 2 hours by the slag method at a temperature of 700°C;

[0051] (4) Grinding the calcined mixture until the specific surface area is 360-400m 2 / kg to obtain solid waste base geopolymer materials.

[0052] The geopolymer gelling material is directly mixed with 70% of the total mass of water and stirred evenly, poured into a mold of 40×40×160, placed in a curing box at 20°C and a r...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
specific surface areaaaaaaaaaaa
compressive strengthaaaaaaaaaa
compressive strengthaaaaaaaaaa
Login to view more

Abstract

The invention discloses a method for preparing a solid waste based geopolymer material from red mud under the cooperation of a slag smoldering method. The method comprises the following steps: 1) uniformly mixing dried and pulverized coal gangues, alkali, sodium silicate, Bayer red mud and melted steel slag to enable the ratio of SiO2 / Al2O3 in a solid substance to be 3.5 to 4.5 and the ratio of Na2O / Al2O3 to be 0.8 to 1.2; 2) calcining a mixture by utilizing the slag smoldering method; 3) pulverizing the calcined mixture to obtain the solid waste based geopolymer material. According to the method disclosed by the invention, after the Bayer red mud, the coal gangues and an alkali metal material are mixed, a mixture is mixed with the melted steel slag; then calcining activation is carried out through the slag smoldering method, so that the activity of silicon and aluminum is improved; a geopolymer gel material which is stirred by directly adding water and naturally cured and molded can be prepared, so that the technical problems that an existing geopolymer gel material prepared from the Bayer red mud needs to be calcined at high temperature, the red mud needs to be subjected to pressfiltering and evaporation drying to remove water, steam pressing or drying molding and the like are needed in a curing process are solved.

Description

technical field [0001] The invention belongs to the field of geopolymer cementitious materials, and in particular relates to a method for preparing solid waste base geopolymers by using the waste heat of converter steel slag and using the stuffy slag method in cooperation with red mud. Background technique [0002] Geopolymers are a new class of high-performance inorganic polymer materials, and they are the most promising class of alkali-activated gelling materials. Due to its special inorganic polycondensation three-dimensional oxide network structure, geopolymer materials have higher high temperature performance and mechanical properties than polymer materials, cement, ceramics and metals in many aspects; on the other hand, the manufacturing process of geopolymer materials The energy consumption and the discharge of three wastes are very low. The material is environmentally friendly and can be recycled and reused. It is a sustainable "green material". The raw materials fo...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): C04B12/00
CPCC04B12/005Y02P40/10
Inventor 李召峰李术才张健林春金齐延海
Owner SHANDONG UNIV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products