Embodiment 1
[0024] Example 1 An adhesive and anti-shedding rubber formula made from the following parts by weight of raw materials:
[0025] Serial number
Component
Dosage / serving
1
Nitrile rubber 4155
100
2
Activated magnesium oxide MgO150
5
3
Anti-aging agent RD
1
4
1
5
DBU Formate
1
6
Carbon black N550
45
7
Carbon black N774
15
8
20
9
Plasticizer RS107
16
10
Sulfur S-80GE
1.5
11
Accelerator CZ
1
12
Accelerator DM
0.5
[0026] Properties of rubber prepared by this formula:
[0027]
[0028] Test result: The bonding strength of fluororubber and fluororesin THV 815 is 4.8N / mm.
Embodiment 2
[0029] Example 2 An adhesive and anti-shedding rubber formula made from the following parts by weight of raw materials:
[0030] Serial number
Component
Dosage / serving
1
Nitrile rubber 4155
100
2
Activated magnesium oxide MgO150
8
3
Anti-aging agent RD
1.5
4
1
5
DBU Formate
1.5
6
Carbon black N550
45
7
Carbon black N774
20
8
15
9
Plasticizer RS107
18
10
Sulfur S-80GE
1.8
11
Accelerator CZ
1
12
Accelerator DM
0.5
[0031] Properties of rubber prepared by this formula:
[0032]
[0033] Test result: The bonding strength of fluororubber and fluororesin THV 815 is 5.6N / mm.
Embodiment 3
[0034] Example 3 An adhesive and anti-shedding rubber formula made from the following parts by weight of raw materials:
[0035] Serial number
Component
Dosage / serving
1
Nitrile rubber 4155
100
2
Activated magnesium oxide MgO150
10
3
Anti-aging agent RD
1
4
1
5
DBU Formate
2
6
Carbon black N550
50
7
Carbon black N774
20
8
Silicon powder 750
20
9
Plasticizer RS107
18
10
Sulfur S-80GE
2
11
Accelerator CZ
1
12
Accelerator DM
0.8
[0036] Properties of rubber prepared by this formula:
[0037]
[0038] Test result: The bonding strength of fluororubber and fluororesin THV 815 is 5.8N / mm.
PUM
Property | Measurement | Unit |
---|---|---|
Adhesive strength | aaaaa | aaaaa |
Adhesive strength | aaaaa | aaaaa |
Adhesive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com