The production method of sodium silicate
A production method and technology of sodium silicate, applied in the direction of silicate, alkali metal silicate, etc., can solve problems such as large energy consumption and environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0055] 1) Provide waste alkali solution, quartz sand and fuel oil produced during alkali washing in the process of producing cyclohexanone by cyclohexane oxidation method for future use.
[0056] 2) The content of Na element recorded in the spent alkali solution by element analysis is 8.3%, and the content of Si element in the quartz sand is 46.1%; the calorific value of the spent alkali solution is 1789kcal / kg, and the heat value of fuel oil is measured by a calorimeter. The value is 10980kcal / kg.
[0057] 3) Mix 1 t of spent alkali solution and 0.1095 t of quartz sand to obtain a mixed solution for later use.
[0058] 4) Add 0.3615t of fuel oil to the mixture prepared in step 3), incinerate in an incinerator, incinerate at 1410°C to 1520°C for 8 hours, and obtain 0.221t of sodium silicate solid after cooling. The purity is 98.4%.
[0059] Among them, t represents the unit: tons.
Embodiment 2
[0061] 1) Provide waste alkali solution, quartz sand and fuel oil produced during alkali washing in the process of producing cyclohexanone by cyclohexane oxidation method for future use.
[0062] 2) The content of Na element recorded in the spent alkali solution by element analysis is 16.5%, and the content of Si element in the quartz sand is 43.5%; the calorific value of the spent alkali solution is 3421kcal / kg, and the heat value of fuel oil is measured by a calorimeter. The value is 10980kcal / kg.
[0063] 3) Mix 1 t of spent alkali solution and 0.1004 t of quartz sand to obtain a mixed solution for later use.
[0064] 4) Add 0.4362t of fuel oil to the mixture prepared in step 3), incinerate in an incinerator, incinerate at 1410°C to 1520°C for 8 hours, and obtain 0.439t of sodium silicate solid after cooling. The purity is 95.1%.
PUM
Property | Measurement | Unit |
---|---|---|
heating value | aaaaa | aaaaa |
heating value | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com