Embodiment 1
[0060] A car label, such as figure 2 As shown, it includes a plastic shell 1 and a rubber filling body 2 , both of which are cross-shaped, and the middle part of the shell 1 is recessed to form a cavity 11 for injection molding of the filling body 2 . The filling body 2 includes an inner filling body 21 located in the cavity 11 , and a surface filling body 22 pasted on the surface of the inner filling body 21 , and the inner filling body 21 fills the entire cavity 11 . The inner filling body 21 is made of common rubber materials, such as CR and BR.
Embodiment 2
[0062] The surface filler 22 in the first embodiment comprises the following components by weight:
[0063] Neoprene 90 parts;
[0064] 50 parts of EPDM rubber;
[0065] 20 parts of tung oil modified phenolic resin;
[0066] 6 parts of α-pinene resin;
[0067] Brightening agent 4 parts;
[0068] Active magnesium oxide 5 parts;
[0069] Active zinc oxide 2 parts;
[0070] 2 parts stearic acid;
[0071] 2 parts of sulfur;
[0072] 1 part of unflavored DCP;
[0073] Accelerator 1.5 parts, accelerator comprises accelerator TMTD, accelerator MBT, accelerator NS that mass ratio is 3:2:2;
[0074] 4 parts of long afterglow phosphor, the long afterglow phosphor is alkaline earth aluminate series, the particle size is 300 mesh;
[0075] 50 parts of fillers, fillers include light calcium carbonate, white carbon black, polytetrafluoroethylene micropowder with a mass ratio of 3:2:1;
[0076] Pigment 8 parts.
[0077] According to the required color of the rubber material, corre...
Embodiment 3
[0093] The surface filler 22 in the first embodiment comprises the following components by weight:
[0094] Neoprene 100 parts;
[0095] 60 parts of EPDM rubber;
[0096] 25 parts of tung oil modified phenolic resin;
[0097] 9 parts of α-pinene resin;
[0098] Brightening agent 6 parts;
[0099] Active magnesium oxide 7 parts;
[0100] Active zinc oxide 3 parts;
[0101] 3 parts stearic acid;
[0102] 3 parts sulfur;
[0103] 1.5 copies of odorless DCP;
[0104] Accelerator 2 parts, accelerator comprises accelerator TMTD, accelerator MBT, accelerator NS that mass ratio is 3:2:2;
[0105] 5 parts of long afterglow phosphor, the long afterglow phosphor is alkaline earth aluminate series, particle size 300 mesh;
[0106] 60 parts of fillers, fillers include light calcium carbonate, white carbon black, polytetrafluoroethylene micropowder with a mass ratio of 3:2:1;
[0107] Pigment 8 parts.
[0108] According to the required color of the rubber material, corresponding ...