Reagent composition for flotation of lepidolite and preparation method and application of reagent composition
A technology of lepidolite and composition, which is applied in flotation, solid separation and other directions, can solve the problems of complex process flow, loss of lepidolite metal, increased loss of lepidolite, etc., and achieves simple process flow and high recovery rate Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0050] A medicament composition for flotation of iron lepidolite of the present invention, comprises coarse grinding composition and adjustment composition, and wherein coarse grinding composition comprises:: sodium hexametaphosphate, sodium tartrate and neutral 2# (collecting agent), its mass ratio is 40::20::40. The adjustment composition includes sodium hexametaphosphate and oxalic acid, and the mass ratio thereof is 60:40.
[0051] The preparation method of the coarse grinding composition of the present embodiment is:
[0052] (1) Sodium hexametaphosphate is formulated into an aqueous solution of sodium hexametaphosphate with a mass fraction of 10%, sodium tartrate is formulated with an aqueous solution of sodium tartrate with a mass fraction of 10%, and neutral 2# is formulated with a mass fraction of 10%. Neutral 2# aqueous solution.
[0053] (2) The sodium hexametaphosphate aqueous solution, the sodium tartrate aqueous solution and the neutral 2# aqueous solution are ...
Embodiment 2
[0058] A method for flotation iron lepidolite without desliming, its technical process see figure 1 , including the following steps:
[0059] (1) Coarse grinding: choose an iron lepidolite mine in Yichun, Jiangxi. The gangue mainly includes quartz, feldspar and calcite, etc. The raw ore 2 The O grade is 0.7-0.8%, and the desliming amount before on-site flotation is 8-10%. Add 1500 g / t of the rough grinding composition of Example 1 to the above-mentioned raw ore that has not been deslimed, and use ceramic balls as the grinding medium for grinding for 3 minutes to obtain rough ground pulp with a -100 mesh content of more than 80%. , -200 mesh content is about 55%.
[0060] (2) The first rough selection:
[0061] 2.1 Add the coarse ground pulp to the mechanical agitation flotation machine, adjust the pulp concentration to about 35% pulp, and the pH of the pulp is 8.45, and fully stir;