Ultra-fine grain high-strength and high-toughness 600MPa-grade anti-seismic steel bar and preparation method thereof

A technology of anti-seismic steel bars and ultra-fine grains, applied in the field of metallurgy, can solve the problems of unfavorable production cost of 600MPa high-strength steel bars, product market competitiveness, poor matching of anti-seismic properties of produced steel bars, and high production costs, so as to promote pearlite content and increase Passivation of corrosion resistance and improvement of shock resistance

Active Publication Date: 2020-07-28
WUKUN STEEL
View PDF8 Cites 7 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] After the implementation of the GB / T 1499.2-2018 standard, there are currently domestic research reports on the production technology of 600MPa straight anti-seismic steel bars after the implementation of the GB / T 1499.2-2018 standard. ≥0.130wt%, the 600MPa high-strength steel bars that meet the GB / T1499.2-2018 standard for macroscopic metallography, cross-section Vickers hardness, and microstructure are obtained through an appropriate controlled rolling process, and the grain size of the microstructure of the steel bar is mostly controlled at 9.5 to 11.0 , due to the high price of vanadium alloys, the production cost is high. In addition, the anti-seismic performance of steel bars produced by this process is not well matched, which is not conducive to the reduction of production costs of 600MPa high-strength steel bars and the improvement of product market competitiveness.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Ultra-fine grain high-strength and high-toughness 600MPa-grade anti-seismic steel bar and preparation method thereof
  • Ultra-fine grain high-strength and high-toughness 600MPa-grade anti-seismic steel bar and preparation method thereof
  • Ultra-fine grain high-strength and high-toughness 600MPa-grade anti-seismic steel bar and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0021] A preparation method of an ultra-fine-grained, high-strength and tough 600MPa-grade seismic steel bar of the present invention includes molten steel smelting, deoxidation alloying, molten steel refining in an argon station, molten steel casting, billet heating, billet controlled rolling and controlled cooling, and specifically includes the following steps:

[0022] a. Molten steel smelting: use steel scrap, pig iron and molten iron at 125-165kg / t respectively 钢 、30kg / t 钢 ,880~920kg / t 钢 The ratio is loaded into the LD converter, and then the conventional top-bottom compound blowing is carried out, and conventional lime, light-burned dolomite, and magnesite balls are added to make slag, and the amount of lime added is 22-28kg / t. 钢 , the amount of lightly burned dolomite added is 12-16kg / t 钢 , the amount of magnesite balls added is 0.5~1.5kg / t 钢 , the carbon content at the control end point is ≥0.07wt%, and the tapping temperature is ≤1630°C; press 1.0kg / t to the bottom...

Embodiment 1

[0039] a. Molten steel smelting: 125kg / t respectively 钢 、30kg / t 钢 The cold material is loaded into the proportion, and the scrap steel (chemical composition: C 0.18wt%, Si 0.40wt%, Mn 1.25wt%, P 0.028wt%, S 0.020wt% is added to the LD converter with the following mass ratio, and the rest is Fe and Inevitable impurities) and pig iron (chemical composition: C 3.2wt%, Si 0.20wt%, Mn 0.35wt%, P0.075wt%, S 0.022wt%, the rest is Fe and unavoidable impurities); Then press 920kg / t 钢 The proportion of molten iron is loaded into the LD converter with the following temperature and mass ratio of molten iron: molten iron temperature 1300 ° C, molten iron composition C 4.0wt%, Si0.20wt%, Mn 0.40wt%, P 0.085wt%, S 0.020wt% , the rest is Fe and unavoidable impurities; scrap steel, pig iron and molten iron are blended into the LD converter, then conventional top-bottom composite blowing is carried out, and conventional lime, lightly burned dolomite and magnesite balls are added to make slag,...

Embodiment 2

[0051] a. Molten steel smelting: 145kg / t respectively 钢 、30kg / t 钢 The cold material is loaded into the proportion, and the steel scrap (chemical composition: C 0.21wt%, Si 0.55wt%, Mn 1.42wt%, P 0.035wt%, S 0.032wt% is added to the LD converter with the following mass ratio, and the rest is Fe and Inevitable impurities) and pig iron (chemical composition: C 3.3wt%, Si 0.30wt%, Mn 0.45wt%, P0.085wt%, S 0.030wt%, the rest is Fe and unavoidable impurities); Then press 900kg / t 钢 The proportion of molten iron is loaded into the LD converter with the following temperature and mass ratio of molten iron: molten iron temperature 1310 ° C, molten iron composition C 4.2wt%, Si0.32wt%, Mn 0.52wt%, P 0.102wt%, S 0.025wt% , the rest is Fe and unavoidable impurities; scrap steel, pig iron and molten iron are blended into the LD converter, then conventional top-bottom composite blowing is carried out, and conventional lime, lightly burned dolomite and magnesite balls are added to make slag,...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses an ultra-fine grain high-strength and high-toughness 600MPa-grade anti-seismic steel bar and a preparation method thereof. The steel bar comprises, by weight, 0.23 wt%-0.27 wt%of C, 0.45 wt%-0.57 wt% of Si, 1.42 wt%-1.55 wt% of Mn, 0.20 wt%-0.25 wt% of Cr, 0.012 wt%-0.017 wt% of Nb, 0.095 wt%-0.110 wt% of V, less than or equal to 0.040 wt% of S, less than or equal to 0.043wt% of P, less than or equal to 0.0070 wt% of O, 0.0240 wt%-0.0265 wt% of N and the balance Fe and inevitable impurities. The preparation method of the steel bar comprises the procedures of molten steel smelting, deoxidation alloying, molten steel argon station refining, molten steel casting, billet heating and billet controlled rolling and controlled cooling. According to the steel bar and the preparation method, a small amount of silicon-nitrogen alloy is added in the steel-making deoxidation alloying process, the nitrogen content in molten steel is increased, the V / N and Nb / N ratio value in steel is reduced, transfer of V and Nb from a solid solution state to a carbonitride precipitated phase in the rolling process is promoted, a large number of fine dispersed V (C, N) and Nb (C, N) precipitated phases are formed and precipitated, and the phase change temperature is reduced, so that the precipitation strengthening effect of the steel is obviously improved; and according to the method, the production cost is reduced, the anti-seismic property is improved, and the market competitiveness of the product is improved.

Description

technical field [0001] The invention belongs to the technical field of metallurgy, and in particular relates to an ultra-fine-grained high-strength and toughness 600MPa-grade anti-seismic steel bar and a preparation method thereof. Background technique [0002] Hot-rolled ribbed steel bar is the main reinforcement material of reinforced concrete building structure, and it carries the stress and strain of loads such as tensile and compressive stress and strain in the structure. At present, the annual output of hot-rolled ribbed steel bars in my country is about 200 million tons, which is the most widely used steel material in the construction of national economic construction projects. With the continuous development of my country's buildings towards high-rise, long-span and earthquake-resistant structures, the development of fine-grained anti-seismic steel bars with high strength, toughness and excellent comprehensive performance has become one of the important tasks for the...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C22C33/06C21C7/00C21C7/06C21C7/064C21D6/00C21D8/06C21D9/52C22C38/02C22C38/04C22C38/24C22C38/26C22C38/38
CPCC21C7/0006C21C7/06C21C7/064C21D6/002C21D6/005C21D6/008C21D8/065C21D9/525C21D2211/002C21D2211/005C21D2211/009C22C33/06C22C38/001C22C38/002C22C38/02C22C38/04C22C38/24C22C38/26C22C38/38Y02P10/20
Inventor 陈伟邓家木赵宇张卫强黄兴凯杨春雷文玉兵张红斌苏灿东刘林刚段家华
Owner WUKUN STEEL
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products