One-component water-based asphalt paint for damping spring and preparation method thereof

A vibration-absorbing spring, one-component technology, applied in asphalt coatings, coatings, polyester coatings, etc., can solve problems such as ecological environment and human health damage, non-compliance with fugitive emissions, economic losses, etc., and achieve anti-sagging Good performance, reduced volatile organic compounds content, reasonable production process effect

Active Publication Date: 2022-04-19
SHANXI HUABAO NEW MATERIALS CO LTD +1
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, solvent-based asphalt coatings have many shortcomings and disadvantages. They contain a large amount of volatile organic solvents, which will cause great harm to the ecological environment and human health during production, transportation, storage and use. With the promulgation of policies, laws and regulations and the intensification of environmental protection supervision, processing, production and construction enterprises often limit or stop production due to non-compliance with fugitive emissions, causing many economic losses

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • One-component water-based asphalt paint for damping spring and preparation method thereof
  • One-component water-based asphalt paint for damping spring and preparation method thereof
  • One-component water-based asphalt paint for damping spring and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0040] The present invention also provides a kind of preparation method of one-component water-based asphalt paint for damping spring as described above, and concrete steps comprise:

[0041]Preparation of premix: Take the water-based polymer emulsion of the formula amount in a clean batching kettle, start stirring, and slowly add dispersant, wetting agent, defoamer of 1 / 2 of the formula amount, After neutralizing agent with 1 / 3 formula quantity, deionized water with 4 / 5 formula quantity, and drier, increase stirring speed to 800-1000r / min, stir for 20-30min; place in disperser, 400-600r / min Add pigments, inorganic nano fillers and thickening rheological additives under stirring, and then disperse at a high speed of 1000-1200r / min for 10-20min until uniform.

[0042] Slurry Grinding: Grind on a sand mill to a fineness of ≤30 μm before discharging.

[0043] Preparation of finished paint: Slowly add defoamer with 1 / 2 formula quantity, neutralizer with 2 / 3 formula quantity, modi...

Embodiment 1-4

[0046] Weigh the raw materials according to the ratio and dosage in Table 1 below, and process the products according to the preparation methods of Examples 1-4, see Table 1 for details.

[0047] Table 1: Raw material ratio table of embodiment 1-4

[0048]

Embodiment 1

[0051] Take 5 parts of 3AK0274B and 10 parts of ETERKYDW3630 water-based polymer emulsion in a clean batching kettle, start stirring, and slowly add 0.1 part of BYK-190 dispersant, 0.1 part of TRITON X-405 wetting agent, 0.15 After 1 part of Foamex8030 and 0.15 part of Foamex K7 defoamer, 0.2 part of DMAE neutralizer, 41.6 parts of deionized water, 0.5 part of cobalt salt drier, increase the stirring speed to 800r / min, stir for 30min; place in a disperser, 500r Add 1 part of carbon black, 10 parts of nano-calcium carbonate, 0.2 part of RM-8W thickening rheology additive under stirring at 1000 r / min for 20 minutes until uniform. Grind on a sand mill to a fineness of ≤30 μm, then discharge and set aside.

[0052] Take the aforementioned slurry, stir at 300r / min, and slowly add 0.15 parts of Foamex8030 and 0.15 parts of FoamexK7 defoamer, 0.4 parts of DMAE neutralizer, 20 parts of HVE modified asphalt emulsion of Guangzhou Shengmei Material Technology Co., Ltd., 10.4 parts After...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a one-component water-based asphalt paint for damping springs and a preparation method thereof. The asphalt paint comprises the following raw materials in parts by weight: 10-30 parts of water-based high polymer emulsion, 20-50 parts of modified asphalt emulsion , 0.1-0.3 parts of dispersant, 0.1-0.2 parts of wetting agent, 0.5-0.8 parts of defoamer, 1-5 parts of pigment, 2-10 parts of inorganic nano filler, 0.2-0.5 part of thickening rheology additive, medium Blending agent 0.6-1.5 parts, drier 0.5-1.2 parts, deionized water 20-55 parts. The product of the present invention uses water as a solvent, modified asphalt emulsion and water-based polymer emulsion as film-forming substances, which greatly reduces the content of volatile organic compounds. After film formation, the surface of the paint film is smooth, dense and tough, and has good storage stability. Good anti-sagging performance, suitable for dip coating construction process requirements; suitable for large-scale batch production, and the obtained products have stable performance and reliable quality.

Description

technical field [0001] The invention relates to a one-component water-based asphalt paint for damping springs and a preparation method thereof, belonging to the technical field of water-based paints. Background technique [0002] The damping spring is an important component of the underframe of the rail vehicle, which plays a key role in alleviating and reducing the vibration and impact caused by vehicle startup, acceleration and deceleration, and ensuring the smooth and safe operation of the vehicle. This part is in the complex and harsh operating environment such as humidity, high temperature and severe cold all the year round. The traditional protection method is to apply solvent-based asphalt paint, which can meet the requirements of use. However, solvent-based asphalt coatings have many shortcomings and disadvantages. They contain a large amount of volatile organic solvents, which will cause great harm to the ecological environment and human health during production, tr...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09D195/00C09D167/08C09D5/08C09D7/20C09D7/61C09D7/43C09D7/65
CPCC09D195/005C09D5/08C09D7/20C09D7/61C09D7/43C09D7/65C08K2201/011C08K2003/265C08L2205/035C08L2205/025C08L53/02C08L9/06C08L67/08C08L75/04C08K3/26C08K3/36C08K3/04
Inventor 赵洪艳郭燕娥田计青韩连山
Owner SHANXI HUABAO NEW MATERIALS CO LTD