A technology of adsorbent and cross-linking agent, applied in the field of degradable adsorbent and its preparation, can solve the problems of sugar residual sulfur, pollution of the environment, inability to meet the requirements of medicine and food, etc., to improve adsorption performance, reduce raw material cost, and solve residual problems. Effects of sulphur problems
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] A preparation method of a degradable adsorbent, comprising the steps of: adding 0.06 g of activated carbon (activated carbon prepared from bagasse) with a particle size of ≤3 μm into 20 ml of a 5 wt % gelatin aqueous solution, and ultrasonically dispersing it uniformly to obtain solution A,
[0028] Add 20ml of solution A and 0.1g of Span 80 into 80ml of ethyl acetate, mix and emulsify for 2 hours to obtain an emulsion, then add 0.2g of glutaraldehyde dropwise and solidify at room temperature for 2.5 hours, filter, wash with ethanol and water for 4 times, Then vacuum freeze-dry at -10°C to obtain a degradable adsorbent with an average particle size of 61 μm.
Embodiment 2
[0030] A preparation method of a degradable adsorbent, comprising the steps of: adding 0.08 g of activated carbon (activated carbon prepared from bagasse) with a particle diameter of ≤3 μm into 12.5 ml of 8 wt % gelatin aqueous solution, and ultrasonically dispersing it uniformly to obtain solution A,
[0031] Add 12.5ml of solution A and 0.3g of Span 80 into 80ml of toluene, mix and emulsify for 2 hours to obtain an emulsion, then add 0.15g of glutaraldehyde dropwise and solidify at room temperature for 3 hours, filter, wash with ethanol and water for 4 times, and then Vacuum freeze-drying at -15°C yields a degradable adsorbent with an average particle size of 70 μm.
Embodiment 3
[0033] A preparation method of a degradable adsorbent, comprising the steps of: adding 0.07 g of activated carbon (activated carbon prepared from bagasse) with a particle size of ≤3 μm into 16 ml of a gelatin aqueous solution with a mass fraction of 6.5 wt%, and ultrasonically dispersing it uniformly to obtain solution A,
[0034] Add 16ml of solution A and 0.2g of Span 80 into 80ml of liquid paraffin, mix and emulsify for 2 hours to obtain an emulsion, then add 0.17g of glutaraldehyde dropwise and solidify at room temperature for 2.8 hours, filter, wash with ethanol and water for 4 times, and then Vacuum freeze-drying at -13°C yielded a degradable adsorbent with an average particle size of 65 μm.