High alumina slag ball and preparing method thereof
A high-aluminum slag ball, metal aluminum technology, applied in the direction of improving process efficiency, can solve problems such as unsatisfactory kinetic conditions, difficulty in forming silicon or manganese, rising, etc., to achieve excellent spreading and thermal insulation performance, reduction of oxide inclusions, Simple effect of ball forming process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0038] The preparation of aluminum slag ball, embodiment one
[0039] Weigh the qualified raw materials: aluminum powder 385Kg, aluminum slag powder 500Kg, titanium slag powder 35Kg, fluorite powder 25Kg, limestone powder 40Kg, put the above-mentioned weighed raw materials into the drum mixer and mix evenly (15 minutes) , put 50Kg of glass water with a pomi degree of 37 into the uniformly mixed material and mix evenly in a double auger mixer, roll the uniformly mixed material into spherical particles of 10-20mm in a double-roller briquetting machine, Put the spherical particles into the drying equipment with coke as fuel, and dry them with hot air at a temperature of about 200°C for 20-24 hours. After the moisture content of the finished product is less than 0.2%, cool naturally for 10-12 hours, then screen and pack again , Storage.
[0040] The component content of the chemical composition of above embodiment finished product is by weight %:
[0041] Al: 50.57;
[0042] Al...
Embodiment 2
[0051] Weigh the qualified raw materials: aluminum powder 460Kg, aluminum slag powder 200Kg, titanium slag powder 135Kg, fluorite powder 75Kg, limestone powder 115Kg, put the above-mentioned weighed raw materials into the drum mixer and mix evenly (15 minutes) , put 50Kg of glass water with a pomi degree of 37 into the uniformly mixed material and mix evenly in a double auger mixer, roll the uniformly mixed material into spherical particles of 10-20mm in a double-roller briquetting machine, Put the spherical particles into the drying equipment with coke as fuel, and dry them with hot air at a temperature of about 150-200°C for 20-24 hours. After the moisture content of the finished product is less than 0.2%, cool naturally for 10-12 hours and then screen again ,wrap up and store.
[0052] The chemical composition of above embodiment finished product is by weight %:
[0053] Al: 50.37;
[0054] Al 2 o 3 : 12.90;
[0055] TiO 2 : 11.63;
[0056] CaF 2 : 7.36;
[0057] C...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com