Method of preparing protein polypeptide retanning agent
A peptide retanning agent and protein technology, which is applied in the field of preparation of environmentally friendly new protein polypeptide retanning agents, can solve problems such as poor hand feel, hardened cortex, insufficient hydrolysis, etc. stable effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Take 128g of calcium lignosulfonate, add 120mL of water, and stir evenly; dissolve 80g of sodium hydroxide in 160mL of water to form NaOH aqueous solution; control the temperature at about 60°C, add NaOH aqueous solution into the aqueous solution of calcium lignosulfonate, Calcium sulfonate aqueous solution is made into a paste, and then 280g of pigskin chrome leather scraps are gradually added into it, and 85mL of water is added in the middle, the temperature is raised to 100°C, and the reaction is carried out for 6.5h. The chrome leather scraps are all hydrolyzed into an aqueous solution of protein and polypeptide. Due to the presence of calcium lignin sulfonate, the solution is thicker. Cool the water bath to about 30°C, add formic acid solution drop by drop to neutralize the alkaline hydrolyzate until the pH value is 6.8, add about 75mL of formic acid, the neutralization and dropping time is controlled at 2.5-3h, and the protein polypeptide hydrolyzate A is obtained,...
Embodiment 2
[0024] Take 140g of calcium lignosulfonate, add 120mL of water, and stir evenly; dissolve 80g of sodium hydroxide in 160mL of water to form NaOH aqueous solution; control the temperature at about 60°C, add NaOH aqueous solution into the aqueous solution of calcium lignosulfonate, lignin Calcium sulfonate aqueous solution is made into a paste, and then 300g of pigskin chrome leather scraps are gradually added to it, and 100mL of water is added in the middle, the temperature is raised to 105°C, and the reaction is carried out for 7.5h. The chrome leather scraps are all hydrolyzed into protein polypeptide aqueous solution. Due to the presence of calcium lignin sulfonate, the solution is thicker. Cool the water bath to about 30°C, add formic acid solution drop by drop to neutralize the alkaline hydrolyzate until the pH value is 6.5, add about 78mL of formic acid, the neutralization and dropping time is controlled at 2.5-3h, and the protein polypeptide hydrolyzate B is obtained, the...
Embodiment 3
[0026] Take 150g of calcium lignosulfonate, add 120mL of water, and stir evenly; dissolve 80g of sodium hydroxide in 160mL of water to form NaOH aqueous solution; control the temperature at about 60°C, add NaOH aqueous solution into the aqueous solution of calcium lignosulfonate, Calcium sulfonate aqueous solution is made into a paste, and then 320g of pigskin chrome leather scraps are gradually added to it, and 120mL of water is added in the middle, the temperature is raised to 110°C, and the reaction is carried out for 8 hours. The chrome leather scraps are all hydrolyzed into an aqueous solution of protein and polypeptide. Due to the presence of calcium lignin sulfonate, the solution is thicker. Cool the water bath to about 30°C, add formic acid solution drop by drop to neutralize the alkaline hydrolyzate until the pH value is 7.5, add about 70mL of formic acid, the neutralization and dropping time is controlled at 2.5-3h, and the protein polypeptide hydrolyzate C is obtaine...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com