Method for extracting germanium from high-impurity low-grade complex zinc oxide powder
A zinc oxide powder and low-grade technology, applied in the field of germanium extraction, can solve problems affecting the normal operation of industrial production, polluting the ecological environment, and loss of valuable resources, so as to increase constructive production investment, low production cost, and stable product output effect in
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] The chemical composition of raw materials used is shown in Table 2:
[0038] Table 2 Zinc oxide soot chemical composition (%)
[0039] Zn Pb F Cl Ge As 25 12 0.22 0.4 0.015 7 Sb Fe Cu Cd S 0.3 7 0.03 3.04 4.2
[0040] steps:
[0041] A adopts conventional three-stage acid leaching of the above-mentioned zinc oxide dust, and then separates the solid and liquid into the zinc sulfate leaching solution after acid leaching. The leaching solution contains 78 mg / L of germanium and 8000 mg / L of iron, of which Fe 3+ Content 385mg / L;
[0042] B. In the above zinc sulfate solution, add zinc sulfite reducing agent in an amount of 0.5g / L, adjust the pH value of the solution to 1.5, and stir to reduce Fe in the zinc sulfate solution at a temperature of 55°C. 3+ <10mg / L;
[0043] C, in the reducing zinc sulfate solution of above-mentioned B step, by the germanium mass meter contained in the solutio...
Embodiment 2
[0050] The chemical composition of raw materials used is shown in Table 3:
[0051] Table 3 Zinc oxide soot chemical composition (%)
[0052] Zn Pb F Cl Ge As 45 20 0.35 1.0 0.065 8 Sb Fe Cu Cd S 0.74 18 0.06 6.8 6.5
[0053] steps:
[0054] A adopts conventional three-stage acid leaching of the above-mentioned zinc oxide fume, and then separates the solid-liquid to separate the zinc sulfate leaching solution after acid leaching. The leaching solution contains 135 mg / L of germanium and 15000 mg / L of iron, of which Fe 3+ Content 614mg / L;
[0055] B. In the above zinc sulfate solution, add sodium sulfite reducing agent in an amount of 3.5g / L, adjust the pH value of the solution to 0.5, and stir to reduce Fe in the zinc sulfate solution at a temperature of 75°C. 3+ <10mg / L;
[0056] C, in the reducing zinc sulfate solution of above-mentioned B step, by the germanium mass meter contained in the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com