A technology for plastering mortar and building exterior walls, applied in the field of building materials, can solve the problems of difficult construction, high cost, high technical requirements, etc., and achieve the effect of being conducive to on-site construction and operation, and good workability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0014] A preparation method for plastering mortar for building exterior walls, comprising the following steps:
[0015] (1) According to the molar ratio of 1:1, mix polyether silicone oil and maleic anhydride, stir well, add 0.5% p-toluenesulfonic acid of the weight of polyether silicone oil as a catalyst, and add acetone as a solvent, and stir at 90°C React for 3 hours, then vacuumize the reaction product at 110°C, and react for 1 hour at a vacuum of 0.04MPa, and finally add 10% sodium bicarbonate solution to adjust the pH to 7, and then mix with sulfated cow hoof oil according to Compounding at a molar ratio of 1:0.4 to obtain component A for use;
[0016] According to parts by weight, take 60 parts of polyethylene glycol, 8 parts of n-dodecane, 3 parts of component A, 12 parts of toluene diisocyanate and 1 part of glycerol, heat and melt the polyethylene glycol, and then add n-dodecane Alkanes and component A, under the protection of nitrogen, control the temperature at 60...
Embodiment 2
[0020] A preparation method for plastering mortar for building exterior walls, comprising the following steps:
[0021] (1) According to the molar ratio of 1:1, mix polyether silicone oil and maleic anhydride, stir well, add 0.5% p-toluenesulfonic acid of the weight of polyether silicone oil as a catalyst, and add acetone as a solvent, and stir at 90°C React for 3 hours, then vacuumize the reaction product at 110°C, and react for 1 hour at a vacuum of 0.04MPa, and finally add 10% sodium bicarbonate solution to adjust the pH to 7, and then mix with sulfated cow hoof oil according to Compounding at a molar ratio of 1:0.4 to obtain component A for use;
[0022] According to parts by weight, take 40 parts of polyethylene glycol, 10 parts of n-dodecane, 2 parts of component A, 20 parts of toluene diisocyanate and 0.1 part of glycerol, heat and melt the polyethylene glycol, and then add n-dodecane Alkanes and component A, under the protection of nitrogen, control the temperature at...
Embodiment 3
[0026] A preparation method for plastering mortar for building exterior walls, comprising the following steps:
[0027] (1) According to the molar ratio of 1:1, mix polyether silicone oil and maleic anhydride, stir well, add 0.5% p-toluenesulfonic acid of the weight of polyether silicone oil as a catalyst, and add acetone as a solvent, and stir at 90°C React for 3 hours, then vacuumize the reaction product at 110°C, and react for 1 hour at a vacuum of 0.04MPa, and finally add 10% sodium bicarbonate solution to adjust the pH to 7, and then mix with sulfated cow hoof oil according to Compounding at a molar ratio of 1:0.4 to obtain component A for use;
[0028] According to parts by weight, take 90 parts of polyethylene glycol, 5 parts of n-dodecane, 4 parts of component A, 4 parts of toluene diisocyanate and 2 parts of glycerol. After heating and melting the polyethylene glycol, add n-dodecane in sequence Alkanes and component A, under the protection of nitrogen, control the te...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com