A thermosetting powder, corrosion-resistant technology, applied in the direction of powder coatings, anti-corrosion coatings, fire-resistant coatings, etc., can solve the problems of chalking, cracking, peeling, etc., and achieve long-lasting color retention, extended life, and excellent corrosion resistance sexual effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A corrosion-resistant thermosetting powder coating, the main components of the powder coating include by weight: 40 parts of epoxy resin, 5 parts of curing agent, 10 parts of polyester resin, 3 parts of surface additives, 5 parts of phenolic resin, 15 parts of barium sulfate, 1 part of pigment, 5 parts of aluminum powder, 5 parts of carbon powder, 1.5 parts of light stabilizer.
[0016] The light stabilizer is a mixture of carbon black, titanium oxide, rosin glyceride and citric acid in a weight ratio of 2:1:1:2.
[0017] The preparation method of the corrosion-resistant thermosetting powder coating, epoxy resin, curing agent, polyester resin, surface additives, phenolic resin, barium sulfate, colorant, aluminum powder, carbon powder, light stabilizer are added according to the proportioning Stir and mix evenly in a mixer, and then extrude through a twin-screw extruder, press into tablets, cool, crush, and sieve to make a corrosion-resistant thermosetting powder coating...
Embodiment 2
[0020] A corrosion-resistant thermosetting powder coating, the main components of the powder coating include by weight: 30 parts of epoxy resin, 3 parts of curing agent, 8 parts of polyester resin, 2 parts of surface additives, 3 parts of phenolic resin, 10 parts of barium sulfate, 1 part of pigment, 3 parts of aluminum powder, 3 parts of carbon powder, 1.2 parts of light stabilizer.
[0021] The light stabilizer is a mixture of carbon black, titanium oxide, rosin glyceride and citric acid in a weight ratio of 2:1:1:2.
[0022] The preparation method of the corrosion-resistant thermosetting powder coating, epoxy resin, curing agent, polyester resin, surface additives, phenolic resin, barium sulfate, colorant, aluminum powder, carbon powder, light stabilizer are added according to the proportioning Stir and mix evenly in a mixer, and then extrude through a twin-screw extruder, press into tablets, cool, crush, and sieve to make a corrosion-resistant thermosetting powder coating....
Embodiment 3
[0025] A corrosion-resistant thermosetting powder coating, the main components of the powder coating include by weight: 50 parts of epoxy resin, 8 parts of curing agent, 12 parts of polyester resin, 5 parts of surface additives, 8 parts of phenolic resin, 20 parts of barium sulfate, 3 parts of pigment, 8 parts of aluminum powder, 6 parts of carbon powder, 1.8 parts of light stabilizer.
[0026] The light stabilizer is a mixture of carbon black, titanium oxide, rosin glyceride and citric acid in a weight ratio of 2:1:1:2.
[0027] The preparation method of the corrosion-resistant thermosetting powder coating, epoxy resin, curing agent, polyester resin, surface additives, phenolic resin, barium sulfate, colorant, aluminum powder, carbon powder, light stabilizer are added according to the proportioning Stir and mix evenly in a mixer, and then extrude through a twin-screw extruder, press into tablets, cool, crush, and sieve to make a corrosion-resistant thermosetting powder coatin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com