A technology of passivating agent and tailings, which is applied in the field of farmland passivating agent, can solve the problems of wasting resources, polluting the environment, occupying land, etc., and achieves the effects of improving quality, simple preparation process and strong applicability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0044] The preparation steps of passivating agent are as follows:
[0045] (1) Take 15g of molybdenum ore tailings and grind through a 200 mesh sieve, add 30mL, 1mol / L H 2 SO 4 Vibrate in a shaker, filter and separate, dry, and then divide into crucibles, add an equal mass of NaOH to each crucible, heat in a muffle furnace at 823K for 3 hours, take it out to cool naturally, and grind it for use.
[0046] (2) Get 5g of the product that is ground for use in step (1) and add 90mL of water to dissolve it, and get the supernatant by centrifugal filtration, transfer it to a teflon tank, add 5.4g of sodium metaaluminate, 15.75g of water glass, and dissolve it at 343K Stir for 1h;
[0047] (3) Transfer the stirred product in the teflon tank to the reactor, react at 373K for 15 hours, then cool the resulting reaction product to room temperature, filter, wash, and dry, and the obtained powder solid is the farmland passivation agent.
[0048]The prepared farmland passivation agent was...
Embodiment 2
[0056] The preparation steps of passivating agent are as follows:
[0057] (1) Take 15g of molybdenum ore tailings and grind through a 200 mesh sieve, add 30mL, 1mol / L H 2 SO 4 Vibrate in a shaker, filter and separate, dry, and then divide into crucibles, add NaOH to each crucible, heat in a muffle furnace at 873K for 2 hours, take it out to cool naturally, grind it for use, and add NaOH to each crucible The quality of NaOH is that the mass ratio of molybdenum ore tailings to NaOH after drying is 0.85.
[0058] (2) Get 5g of the product that is ground for use in step (1) and add 90mL of water to dissolve it, and get the supernatant by centrifugal filtration, transfer it to a teflon tank, add 5.4g of sodium metaaluminate, 15.75g of water glass, and dissolve it at 333K Stir for 3h;
[0059] (3) Transfer the stirred product in the teflon tank to the reactor, react at 373K for 12 hours, then cool the resulting reaction product to room temperature, filter, wash, and dry, and the...
Embodiment 3
[0068] The preparation steps of passivating agent are as follows:
[0069] (1) Take 15g of molybdenum ore tailings and grind through a 200 mesh sieve, add 30mL, 1mol / L H 2 SO 4 Vibrate in a shaker, filter and separate, dry, and then divide into crucibles, add an equal mass of NaOH to each crucible, heat in a muffle furnace at 823K for 3 hours, take it out to cool naturally, and grind it for use.
[0070] (2) Get 5g of the product that is ground for use in step (1) and add 90mL of water to dissolve it, and get the supernatant by centrifugal filtration, transfer it to a teflon tank, add 5.4g of sodium metaaluminate, 15.75g of water glass, and dissolve it at 343K Stir for 2h;
[0071] (3) Transfer the stirred product in the teflon tank to the reactor, react at 403K for 8 hours, then cool the obtained reaction product to room temperature, filter, wash, and dry, and the obtained powder solid is the farmland passivation agent.
[0072] The prepared farmland passivation agent was ...