An anti-corrosion spraying, outdoor cabinet technology, applied in coatings, powder coatings, polyurea/polyurethane coatings, etc., can solve problems such as poor working environment, hidden dangers in process production, easy corrosion of bases, etc., and achieve excellent anti-corrosion performance. The effect of super strong adhesion and excellent anti-corrosion performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A kind of anticorrosion spraying method for outdoor cabinet base, comprises the following steps:
[0027] (1) Sanding treatment of the base: place the base of the outdoor cabinet in a sanding room to ensure that the surface of the base is free of dirt, and perform sanding treatment; then immerse it in a degreasing solution to remove oil stains and dust on the surface, and use Rinse with clean water and dry;
[0028] (2) Phosphating treatment: Put the dried outdoor cabinet base into the phosphating pool for soaking treatment, take it out after soaking for 8 minutes, and then dry it. The baking temperature is 110°C and the baking time is 10 minutes; among them, the phosphating solution It is composed of the following parts by mass: 30 parts of 80% phosphoric acid, 30 parts of phosphate, 20 parts of molybdate, 15 parts of citric acid, 5 parts of surfactant, 5 parts of octylphenol polyoxyethylene ether, and 10 parts of accelerator share;
[0029] (3) Hanging: After pastin...
Embodiment 2
[0034] A kind of anticorrosion spraying method for outdoor cabinet base, comprises the following steps:
[0035] (1) Sanding treatment of the base: place the base of the outdoor cabinet in a sanding room to ensure that the surface of the base is free of dirt, and perform sanding treatment; then immerse it in a degreasing solution to remove oil stains and dust on the surface, and use Rinse with clean water and dry;
[0036] (2) Phosphating treatment: put the dried base of the outdoor cabinet into the phosphating pool for soaking treatment, take it out after soaking for 9 minutes, and then dry it. The baking temperature is 120°C, and the baking time is 12 minutes; among them, the phosphating solution It consists of the following parts by mass: 40 parts of 85% phosphoric acid, 20 parts of phosphate, 30 parts of molybdate, 10 parts of citric acid, 7 parts of surfactant, 8 parts of octylphenol polyoxyethylene ether, and 15 parts of accelerator share;
[0037] (3) Hanging: After p...
Embodiment 3
[0042] An anti-corrosion spraying method for an outdoor cabinet base, comprising the following steps:
[0043] (1) Sanding treatment of the base: place the base of the outdoor cabinet in the sanding room to ensure that the surface of the base is free of dirt, and then perform sanding treatment; then immerse it in a degreasing solution to remove oil stains and ash on its surface, and use Rinse with clean water and then dry;
[0044] (2) Phosphating treatment: put the dried outdoor cabinet base into a phosphating tank for soaking treatment, soak it for 10 minutes, take it out, and then dry it. The baking temperature is 140°C and the baking time is 15 minutes; It is composed of the following substances in parts by mass: 50 parts of 80% phosphoric acid, 50 parts of phosphate, 30 parts of molybdate, 20 parts of citric acid, 10 parts of surfactant, 10 parts of octylphenol polyoxyethylene ether, and 20 parts of accelerator share;
[0045] (3) Hanging on the top: After attaching the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology