A kind of air filter paper and nanotechnology, which is applied in the field of nano air filter paper and its preparation, can solve the problems of short service life, low strength, loose paper quality, etc., and achieve the effect of long service life, good water resistance and compact paper quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] Take 60 parts of alkali-treated cotton linter pulp, 15 parts of alkali-free glass fiber chopped strands, 10 parts of nano-carbon fiber polymer, 10 parts of silica filler, 1.5 parts of modified starch light fat calcium carbonate, silicate fiber 2 parts, 5 parts of polyimide fiber, 5 parts of PET and pp composite short fiber, 5 parts of styrene-acrylic emulsion, 0.2 parts of organotin stabilizer, 40 parts of thermoplastic phenolic resin, 80 parts of industrial methanol, polyethyleneimine solution 3 parts, carry out the preparation of nano air filter paper according to the following steps:
[0029] a) Take alkali-treated cotton linter pulp, silica filler, modified starch light fat calcium carbonate, PET and pp composite staple fiber, pulp it through a pulper, and then refine it through a refiner to produce The beating degree of pulp is 15 degrees;
[0030] b) Take nano-carbon fiber polymer, alkali-free glass fiber chopped strands, silicate fiber, polyimide fiber, and use ...
Embodiment 2
[0036] Take 70 parts of alkali-treated cotton linter pulp, 18 parts of alkali-free glass fiber chopped strands, 15 parts of nano-carbon fiber polymer, 12 parts of silica filler, 3 parts of modified starch light fat calcium carbonate, silicate fiber 6 parts, 10 parts of polyimide fiber, 8 parts of PET and pp composite short fiber, 8 parts of styrene-acrylic emulsion, 0.3 parts of organotin stabilizer, 15 parts of thermoplastic phenolic resin, 100 parts of industrial methanol, polyethyleneimine solution 4 parts, carry out the preparation of nano air filter paper according to the following steps:
[0037] a) Take alkali-treated cotton linter pulp, silica filler, modified starch light fat calcium carbonate, PET and pp composite staple fiber, pulp it through a pulper, and then refine it through a refiner to produce The beating degree of pulp is 17 degrees;
[0038] b) Take nano-carbon fiber polymer, alkali-free glass fiber chopped strands, silicate fiber, and polyimide fiber, and ...
Embodiment 3
[0044]Take 80 parts of alkali-treated cotton linter pulp, 20 parts of alkali-free glass fiber chopped strands, 20 parts of nano-carbon fiber polymer, 15 parts of silica filler, 5 parts of modified starch light fat calcium carbonate, silicate fiber 10 parts, 15 parts of polyimide fiber, 10 parts of PET and pp composite staple fiber, 10 parts of styrene-acrylic emulsion, 0.4 part of organotin stabilizer, 50 parts of thermoplastic phenolic resin, 120 parts of industrial methanol, polyethyleneimine solution 5 parts, carry out the preparation of nano air filter paper according to the following steps:
[0045] a) Take alkali-treated cotton linter pulp, silica filler, modified starch light fat calcium carbonate, PET and pp composite staple fiber, pulp it through a pulper, and then refine it through a refiner to produce The beating degree of pulp is 19 degrees;
[0046] b) Take nano-carbon fiber polymer, alkali-free glass fiber chopped strands, silicate fiber, and polyimide fiber, an...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle size | aaaaa | aaaaa |
| height | aaaaa | aaaaa |
| water absorption | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More